WO2023191081A1 - ポリオレフィン系樹脂発泡体及び成形体 - Google Patents
ポリオレフィン系樹脂発泡体及び成形体 Download PDFInfo
- Publication number
- WO2023191081A1 WO2023191081A1 PCT/JP2023/013652 JP2023013652W WO2023191081A1 WO 2023191081 A1 WO2023191081 A1 WO 2023191081A1 JP 2023013652 W JP2023013652 W JP 2023013652W WO 2023191081 A1 WO2023191081 A1 WO 2023191081A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- polyolefin resin
- variation
- foam
- coefficient
- less
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/32—Layered products comprising a layer of synthetic resin comprising polyolefins
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B5/00—Layered products characterised by the non- homogeneity or physical structure, i.e. comprising a fibrous, filamentary, particulate or foam layer; Layered products characterised by having a layer differing constitutionally or physically in different parts
- B32B5/18—Layered products characterised by the non- homogeneity or physical structure, i.e. comprising a fibrous, filamentary, particulate or foam layer; Layered products characterised by having a layer differing constitutionally or physically in different parts characterised by features of a layer of foamed material
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J9/00—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof
- C08J9/04—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof using blowing gases generated by a previously added blowing agent
- C08J9/06—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof using blowing gases generated by a previously added blowing agent by a chemical blowing agent
Definitions
- the present invention relates to a polyolefin resin foam and a molded article.
- Polyolefin resin foams have excellent moldability due to the characteristics of the resin used, and the foams after molding are used for cushioning materials for vehicle interior materials and the like.
- polyolefin resin foams retain odors resulting from the materials used and by-products generated during the production process, which may cause a problem as interior odor after being installed in a vehicle. For example, surveys of dissatisfaction with the purchase of a new car show that many users find the smell inside the car unpleasant.
- Patent Document 1 As a method for reducing the odor of polyolefin resin foams, for example, a method using basic magnesium (Patent Document 1) is known. In addition to this, there are methods using deodorizing agents (Patent Document 2), methods using activated carbon, etc. (Patent Document 3), methods using carbon black, etc. (Patent Document 4), and methods using zeolite (Patent Document 5). , a method using roasted alum and zeolite (Patent Document 6), and the like are known.
- JP 2021-169549 Publication Japanese Patent Application Publication No. 2021-172676 Japanese Patent Application Publication No. 11-60774 Japanese Patent Application Publication No. 11-263863 Patent No. 6832112 Japanese Patent Application Publication No. 2002-12690
- an object of the present invention is to provide a polyolefin resin foam that can reduce odor generation compared to conventional foams, and a molded article obtained by molding the polyolefin resin foam.
- the present inventors determined that the coefficients of variation of the cell diameter in the width direction (TD), the cell diameter in the thickness direction (ZD), the cell flatness, and the cell area were set to below a certain level, and that metal oxides and metals were The inventors have discovered that the above-mentioned problems can be solved by a polyolefin resin foam containing at least a certain amount of at least one filler selected from hydroxides, and have completed the present invention. That is, the present invention includes the following [1] to [9].
- the coefficient of variation of the cell diameter in the width direction (TD) and the cell diameter in the thickness direction (ZD) per 50 cells contained in the foam are each 0.38 or less, and the coefficient of variation of the cell oblateness is 0.45 or less, the coefficient of variation of cell area is 0.65 or less, and contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is is 0.3% by mass or more based on the total amount of the polyolefin resin foam.
- the coefficient of variation of the cell diameter in the width direction (TD) and the coefficient of variation of the cell diameter in the thickness direction (ZD) per 50 cells contained in the foam are each 0.38 or less, and the coefficient of variation of the cell oblateness is 0.45 or less, the coefficient of variation of the bubble area is 0.65 or less, It contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is 0.4 parts by mass or more based on 100 parts by mass of the polyolefin resin. , polyolefin resin foam. [10] The polyolefin resin foam according to [9] above, wherein the coefficient of variation of the cell diameter in the width direction (TD) is 0.35 or less.
- the polyolefin resin foam of the present invention has a coefficient of variation in the cell diameter in the width direction (TD) and a coefficient of variation in the cell diameter in the thickness direction (ZD) of 0.38 or less per 50 cells contained in the foam. , the coefficient of variation of cell flatness is 0.45 or less, and the coefficient of variation of cell area is 0.65 or less.
- the polyolefin resin foam contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is relative to the total amount of the polyolefin resin foam. It is 0.3% by mass or more.
- the polyolefin resin foam contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is based on 100 parts by mass of the polyolefin resin. The amount may be 0.4 parts by mass or more.
- the polyolefin resin foam of the present invention (hereinafter also simply referred to as foam) has a sheet-like shape.
- TD means Transverse Direction, which is a direction perpendicular to the extrusion direction (MD: Machine Direction) of the foam, and means the width direction of the foam.
- ZD means Thickness Direction, which is a direction perpendicular to both MD and TD, and is the thickness direction of the foam.
- the polyolefin resin foam of the present invention can reduce odor generation. Although the reason for this is not certain, it is presumed as follows. As described above, in the polyolefin resin foam of the present invention, the coefficient of variation of the cell diameter in TD and ZD, the coefficient of variation of the cell flatness, and the coefficient of variation of the cell area are below a certain value. This means that the shapes of the plurality of bubbles (cells) present in the foam are highly uniform. It is thought that if the shape of the plurality of bubble cells is highly uniform, the distribution of the resin constituting the foam will also be more uniform, and odor will be reduced.
- the polyolefin resin foam of the present invention contains at least a certain amount of at least one filler selected from metal oxides and metal hydroxides. This accelerates the decomposition of the blowing agent (for example, a thermally decomposable blowing agent such as azodicarbonamide) used in the production of the polyolefin resin foam, and reduces the amount of blowing agent residue that causes odor.
- the polyolefin resin foam of the present invention effectively reduces odor due to both the high uniformity of the shape of the plurality of cells and the fact that it contains a certain amount or more of a specific filler. It is thought that
- the polyolefin resin foam of the present invention has a coefficient of variation of cell diameter in the width direction (TD) of 0.38 or less per 50 cells contained in the foam.
- TD width direction
- the coefficient of variation of the TD cell diameter in the foam is preferably 0.35 or less, more preferably 0.30 or less, and still more preferably 0.25 or less.
- the coefficient of variation of the cell diameter in TD is preferably 0.1 or more from a practical viewpoint of manufacturing. Note that the coefficient of variation of the bubble diameter in TD is measured as follows.
- the polyolefin resin foam of the present invention has a coefficient of variation of cell diameter in the thickness direction (ZD) per 50 cells contained in the foam of 0.38 or less.
- ZD thickness direction
- the coefficient of variation of the ZD cell diameter in the foam is preferably 0.33 or less, more preferably 0.28 or less, and even more preferably 0.23 or less.
- the coefficient of variation of the bubble diameter of ZD is preferably 0.1 or more from a practical viewpoint of manufacturing. Note that the coefficient of variation of the bubble diameter of ZD is measured as follows.
- the polyolefin resin foam of the present invention has a coefficient of variation of cell flatness per 50 cells contained in the foam of 0.45 or less.
- the coefficient of variation of cell flatness in the foam is preferably 0.40 or less, more preferably 0.35 or less, and even more preferably 0.30 or less.
- the coefficient of variation of the cell oblateness is preferably 0.2 or more from a practical viewpoint of manufacturing. Note that the coefficient of variation of the cell oblateness is measured as follows.
- the polyolefin resin foam of the present invention has a coefficient of variation of cell area per 50 cells contained in the foam of 0.65 or less.
- the coefficient of variation of the cell area in the foam is preferably 0.60 or less, more preferably 0.55 or less, and even more preferably 0.50 or less.
- the coefficient of variation of the bubble area is preferably 0.25 or more from a practical viewpoint of manufacturing. Note that the coefficient of variation of the bubble area is measured as follows.
- a cross section of the polyolefin resin foam cut in the thickness direction along the TD direction was photographed with a magnification of 200 times using a digital microscope, and the TD bubble diameter and ZD bubble diameter were determined for 50 bubbles. are measured respectively, and the area of 50 bubbles is determined based on the following formula.
- Bubble area (Pi) x (TD bubble diameter/2) x (ZD bubble diameter/2) Then, based on the 50 bubble areas thus obtained, the average bubble area and the standard deviation of the bubble areas are determined. Then, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble area by the average bubble area becomes the coefficient of variation of the bubble area.
- Coefficient of variation of bubble area Standard deviation of bubble area / Average bubble area
- the method of keeping each coefficient of variation below a certain level as described above is not particularly limited, but includes, for example, a method of applying the foam manufacturing method described below.
- the polyolefin resin foam of the present invention contains at least one filler selected from metal oxides and metal hydroxides in an amount of 0.3% by mass or more based on the total amount of the polyolefin resin foam. Thereby, the odor generated from the foam can be reduced.
- the filler is at least one selected from metal oxides and metal hydroxides, and is preferably a metal oxide from the viewpoint of easily reducing odor.
- the metal oxide include magnesium oxide, titanium oxide, silicon oxide, zinc oxide, and aluminum oxide, and among them, magnesium oxide is preferred from the viewpoint of odor reduction.
- the metal hydroxide include magnesium hydroxide, aluminum hydroxide, iron hydroxide, and magnesium hydroxide is preferred. Among these fillers, magnesium oxide is particularly preferred from the viewpoint of odor reduction.
- One type of filler may be used alone, or two or more types may be used in combination.
- the filler content in the polyolefin resin foam is 0.3% by mass or more based on the total amount of the polyolefin resin foam.
- the filler content is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 0.9% by mass, based on the total amount of the polyolefin resin foam.
- % by mass or more and from a practical viewpoint of production, preferably 10% by mass or less, more preferably 5% by mass or less, still more preferably 2% by mass or less, and still more preferably 1% by mass. % or less.
- the content of the filler in the polyolefin resin foam may be 0.4 parts by mass or more based on 100 parts by mass of the polyolefin resin.
- the content of the filler is 0.4 parts by mass or more, the residue of the blowing agent such as azodicarbonamide is less likely to remain in the foam, and odor is less likely to occur.
- the content of the filler is preferably 0.6 parts by mass or more, more preferably 1.0 parts by mass or more, based on 100 parts by mass of the polyolefin resin. From this viewpoint, it is preferably 10 parts by mass or less.
- the polyolefin resin foam of the present invention contains a polyolefin resin.
- the polyolefin resin include polypropylene resin, polyethylene resin, thermoplastic olefin elastomer (TPO), and ethylene- ⁇ -olefin copolymer rubber.
- TPO thermoplastic olefin elastomer
- ethylene- ⁇ -olefin copolymer rubber it is preferable to contain at least a polypropylene resin from the viewpoint of ensuring a certain mechanical strength of the foam and ensuring good moldability even at high temperatures.
- the polyolefin resin may include at least one selected from polyethylene resins, olefin thermoplastic elastomers, and ethylene- ⁇ -olefin copolymer rubbers in addition to polypropylene resins. preferable.
- the polypropylene resin is not particularly limited, and examples include propylene homopolymers (homopolypropylene) and copolymers of propylene and other olefins.
- the copolymer of propylene and other olefin may be a block copolymer, a random copolymer, or a random block copolymer, but a random copolymer (random polypropylene) is preferable.
- Examples of other olefins copolymerized with propylene include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, etc. -Olefins, among which ethylene is preferred. Therefore, as the random polypropylene, ethylene-propylene random copolymer is more preferable.
- propylene homopolymer (homopolypropylene) or random polypropylene is preferred from the viewpoint of moldability, and random polypropylene is more preferred.
- One type of polypropylene resin may be used alone or two or more types may be used in combination.
- the polypropylene resin preferably has a melt flow rate (hereinafter also referred to as "MFR") of 0.1 to 20 g/10 minutes at 230°C.
- MFR melt flow rate
- the MFR of the polypropylene resin is preferably 0.3 to 15 g/10 minutes.
- the content of the polypropylene resin is preferably 15 to 90% by mass based on the total amount of resin constituting the foam.
- the content of the polypropylene resin is more preferably 30 to 85% by mass, and even more preferably 50 to 80% by mass.
- the polyolefin resin in the present invention contains a polyethylene resin in addition to a polypropylene resin. This allows the flexibility of the foam to be further improved.
- the polyethylene resin is not particularly limited and includes, for example, low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, and the like, with linear low-density polyethylene being preferred.
- linear low density polyethylene include ethylene/1-butene copolymer, ethylene/1-hexene copolymer, ethylene/4-methyl-1-pentene copolymer, and ethylene/1-octene copolymer. Can be mentioned.
- the linear low density polyethylene is polyethylene having a density of 0.880 to 0.940 g/cm 3 , preferably 0.900 to 0.930 g/cm 3 .
- the density is measured in accordance with JIS K 7112.
- the melt flow rate (MFR) of the polyethylene resin at 190°C is preferably 0.5 to 20 g/10 minutes, more preferably 1 to 15 g/10 minutes, and 1. More preferably 5 to 12 g/10 minutes.
- the content of the polyethylene resin is preferably 10 to 50% by mass based on the total amount of resin components constituting the foam.
- the content of polyethylene resin is preferably 10 to 50% by mass based on the total amount of resin components constituting the foam.
- the content of polyethylene resin is more preferably 15 to 45% by mass.
- the polyolefin resin in the present invention preferably contains a thermoplastic olefin elastomer (TPO) in addition to the polypropylene resin. This allows the flexibility of the foam to be further improved.
- TPO examples include blend type elastomers and dynamic crosslinking type elastomers.
- a blended elastomer is produced by blending a polyolefin resin with a rubber component.
- the rubber component may be partially crosslinked before blending with the polyolefin resin.
- a dynamically crosslinked elastomer is produced by crosslinking the rubber component while mixing the polyolefin resin and the rubber component.
- Rubber components to be blended with the polyolefin resin include, for example, ethylene-propylene copolymer (EPR), ethylene-propylene-diene copolymer (EPDM), acrylonitrile-butadiene rubber (NBR), natural rubber (NR), and isobutylene.
- EPR ethylene-propylene copolymer
- EPDM ethylene-propylene-diene copolymer
- NBR acrylonitrile-butadiene rubber
- NR natural rubber
- isobutylene isobutylene.
- the content of TPO is preferably 10 to 60% by mass based on the total amount of resin constituting the foam. By setting the TPO content to 10% by mass or more, the flexibility of the foam can be further improved. Furthermore, by setting the content to 60% by mass or less, the mechanical strength of the foam can be improved. From the above viewpoint, the content of TPO is more preferably 15 to 45% by mass.
- the polyolefin resin in the present invention preferably contains an ethylene- ⁇ -olefin copolymer rubber in addition to the polypropylene resin. This allows the flexibility of the foam to be further improved.
- the ethylene- ⁇ -olefin copolymer rubber is preferably an amorphous or low-crystalline rubbery material in which two or more olefin monomers are substantially randomly copolymerized.
- the ⁇ -olefins used in the ethylene- ⁇ -olefin copolymer rubber include propylene, 1-butene, 2-methylpropylene, 3-methyl-1-butene, 1-pentene, 1-hexene, and 4-methyl- Examples include one or more ⁇ -olefins having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, such as 1-pentene and 1-octene.
- the ethylene- ⁇ -olefin copolymer rubber may have other monomer units in addition to ethylene units and ⁇ -olefin units.
- monomers forming the other monomer units include conjugated dienes having 4 to 8 carbon atoms, non-conjugated dienes having 5 to 15 carbon atoms, vinyl ester compounds, unsaturated carboxylic acid esters, unsaturated carboxylic acids, and the like.
- conjugated diene having 4 to 8 carbon atoms include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc. It will be done.
- non-conjugated dienes having 5 to 15 carbon atoms include dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-dicyclooctadiene, 7-methyl-1,6-octadiene, -vinyl-2-norbornene and the like.
- vinyl ester compound examples include vinyl acetate.
- unsaturated carboxylic acid ester include methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate.
- unsaturated carboxylic acids include acrylic acid and methacrylic acid.
- These monomers can be used alone or in combination of two or more.
- nonconjugated dienes having 5 to 15 carbon atoms are preferred, and from the viewpoint of easy availability, 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene (DCPD) are more preferred.
- DCPD dicyclopentadiene
- ethylene- ⁇ -olefin copolymer rubbers ethylene-propylene copolymer (EPR) and ethylene-propylene-diene copolymer (EPDM) are preferred, and among them, EPDM is more preferred.
- the content of the ethylene- ⁇ -olefin copolymer rubber is preferably 3 to 30% by mass based on the total amount of resin constituting the foam.
- the content of the ethylene- ⁇ -olefin copolymer rubber is more preferably 5 to 15% by mass.
- polyolefin resin resin components other than those mentioned above may be used. Specifically, examples include ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-(meth)alkyl acrylate copolymer, and modified copolymer copolymerized with maleic anhydride. It will be done.
- the foam may also contain resins other than polyolefin resins, such as styrene thermoplastic elastomers, as long as they do not impede the effects of the present invention.
- the content of resins other than polyolefin resins is, for example, 25% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 0% by mass, based on the total amount of resin components. %.
- the foam of the present invention is formed by foaming a foamable composition containing the above polyolefin resin and filler, and is preferably formed by crosslinking and foaming.
- the foamable composition usually contains a foaming agent as an additive, and preferably also contains a crosslinking aid, an antioxidant, and the like.
- blowing agent a thermally decomposable blowing agent
- an organic or inorganic chemical blowing agent having a decomposition temperature of about 160 to 270° C.
- organic blowing agents include azo compounds such as azodicarbonamide, azodicarboxylic acid metal salts (barium azodicarboxylate, etc.), azobisisobutyronitrile, nitroso compounds such as N,N'-dinitrosopentamethylenetetramine
- examples include hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonyl hydrazide), toluenesulfonyl hydrazide, and semicarbazide compounds such as toluenesulfonyl semicarbazide.
- inorganic blowing agents include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, anhydrous monosodium citric acid, and the like.
- azo compounds and nitroso compounds are preferred from the viewpoint of obtaining fine bubbles, economy, and safety, and azodicarbonamide, azobisisobutyronitrile, N,N'-dinitrosopentamethylene Tetramine is more preferred, and azodicarbonamide is particularly preferred.
- the content of the thermally decomposable blowing agent in the foamable composition is preferably 1 to 20 parts by mass per 100 parts by mass of the polyolefin resin, so that the foam can be properly foamed without bursting the cells of the foam. It is more preferably 15 parts by weight, and even more preferably 5 to 10 parts by weight.
- Crosslinking aid As a crosslinking aid, a polyfunctional monomer can be used.
- trifunctional (meth)acrylate compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate, triallyl trimellitate, triallyl 1,2,4-benzenetricarboxylic acid, triallylisocyanurate, etc.
- difunctional compounds such as 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, neopentyl glycol dimethacrylate, etc.
- Examples include meth)acrylate compounds, compounds having two functional groups in one molecule such as divinylbenzene, diallyl phthalate, diallyl terephthalate, and diallyl isophthalate, ethylvinylbenzene, lauryl methacrylate, and stearyl methacrylate.
- the crosslinking aids can be used alone or in combination of two or more. Among the above, (meth)acrylate compounds are preferred.
- the content of the crosslinking aid in the foamable composition is preferably 0.2 to 20 parts by weight per 100 parts by weight of the polyolefin resin. When this content is 0.2 parts by mass or more, it becomes easier to adjust the degree of crosslinking to a desired level when foaming the foamable composition. Further, when the amount is 20 parts by mass or less, the degree of crosslinking imparted to the foamable composition can be easily controlled.
- the content of the crosslinking aid is more preferably 0.5 to 10 parts by weight, and even more preferably 1 to 8 parts by weight, based on 100 parts by weight of the polyolefin resin.
- antioxidants examples include phenolic antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, amine-based antioxidants, etc. Among these, phenolic antioxidants, phosphorus-based antioxidants, etc. It is preferable to use a phenolic antioxidant, and it is more preferable to use a phenolic antioxidant and a phosphorus antioxidant together. Antioxidants can be used alone or in combination of two or more.
- the content of the antioxidant in the foamable composition is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the polyolefin resin.
- the foam composition may contain other additives other than those mentioned above, such as foaming aids, flame retardants, metal damage inhibitors, antistatic agents, stabilizers, and pigments, as necessary.
- the expansion ratio of the polyolefin resin foam of the present invention is preferably 8 cm 3 /g or more, more preferably 10 cm 3 /g or more, and even more preferably 15 cm 3 /g or more.
- the expansion ratio of the foam is preferably 30 cm 3 /g or less, more preferably 28 cm 3 /g or less, still more preferably 25 cm 3 /g or less, from the viewpoint of ensuring a certain mechanical strength.
- the foaming ratio in the present invention refers to the reciprocal of the density of the foam sheet measured in accordance with JIS K7222.
- the apparent density of the polyolefin resin foam of the present invention is preferably 0.03 g/cm 3 or more, more preferably 0.04 g/cm 3 or more from the viewpoint of ensuring a constant mechanical strength. Further, the apparent density of the foam is preferably 0.13 g/cm 3 or less, more preferably 0.10 g/cm 3 or less, from the viewpoint of improving flexibility.
- the polyolefin resin foam of the present invention is preferably a crosslinked product.
- the degree of crosslinking (%) representing the degree of crosslinking of the foam is preferably 30 to 60%.
- the degree of crosslinking is within the above range, the foam will have excellent flexibility while maintaining good mechanical strength. From these viewpoints, the degree of crosslinking (%) of the foam sheet is more preferably 35 to 55%.
- the thickness of the polyolefin resin foam of the present invention is preferably 0.5 to 5 mm, more preferably 1 to 4 mm. When the thickness is within these ranges, the molded product formed from the foam can be suitably used as a vehicle interior material.
- the MD tensile strength at 120°C of the polyolefin resin foam of the present invention is preferably 0.15 MPa or more, more preferably 0.25 MPa or more, from the viewpoint of uniformly molding the foam, and , preferably 3 MPa or less, more preferably 1 MPa or less.
- the TD tensile strength at 120°C of the polyolefin resin foam of the present invention is preferably 0.07 MPa or more, more preferably 0.10 MPa or more, from the viewpoint of uniformly molding the foam, and , preferably 2 MPa or less, more preferably 1 MPa or less.
- the MD tensile elongation at 120°C of the polyolefin resin foam of the present invention is preferably 250% or more, more preferably 300% or more, from the viewpoint of making the material less likely to break during molding such as vacuum forming. and more preferably 400% or more.
- the MD tensile elongation at 120° C. of the polyolefin resin foam is preferably 1000% or less from a practical manufacturing standpoint.
- the TD tensile elongation at 120°C of the polyolefin resin foam of the present invention is preferably 160% or more, more preferably 200% or more, from the viewpoint of making the material less likely to break during molding such as vacuum forming. and more preferably 300% or more.
- the TD tensile elongation at 120° C. of the polyolefin resin foam is preferably 1000% or less from a practical manufacturing standpoint.
- the tensile strength and tensile elongation at 120° C. of the foam can be adjusted within the above-mentioned predetermined ranges by adjusting the type of resin component. It can also be adjusted by adjusting the expansion ratio, degree of crosslinking, etc.
- the heating dimensional change rate in MD at 120°C of the polyolefin resin foam of the present invention is preferably -8 to 8%, more preferably -7 to 7, from the viewpoint of improving moldability in vacuum forming and the like. %, more preferably -5 to 5%.
- the heating dimensional change rate of TD at 120°C of the polyolefin resin foam of the present invention is preferably -7 to 7%, more preferably -6 to 6% from the viewpoint of improving moldability in vacuum forming etc. %, more preferably -4 to 4%.
- Method for producing polyolefin resin foam It is formed by foaming a foamable composition containing a polyolefin resin, a filler, and a foaming agent, and is preferably formed by crosslinking and foaming.
- the polyolefin resin foam of the present invention is not particularly limited, but it can be produced by heating a foamable sheet made of a foamable composition containing a polyolefin resin, a filler, and a foaming agent to foam the foaming agent.
- the foamable sheet is crosslinked, and the crosslinked foamable sheet is heated to foam.
- the foamable composition may contain a crosslinking aid, an antioxidant, and other additives as necessary.
- the foamable composition is produced by using at least the following components as raw materials: a polyolefin resin, a filler masterbatch, and a blowing agent, and melting and kneading these components.
- the filler masterbatch is produced by melt-kneading the filler of the present invention and a polyolefin resin, and preferably has a pellet-like shape.
- the content of the filler in the filler masterbatch is preferably 10 to 50% by mass, more preferably 20 to 30% by mass, from the viewpoint of making it easier to obtain a foam whose coefficient of variation is below a certain level.
- crosslinking aids, antioxidants, and other additives can be used as necessary.
- Step (1) After supplying each raw material of the foamable composition to a kneading device and kneading, obtaining a sheet-like foamable composition
- Step (2) Adding the foamable composition obtained in step (1) to the foamable composition obtained in step (1).
- Step (3) Step of heating the foamable composition crosslinked in step (2) to a temperature higher than the decomposition temperature of the blowing agent to foam it to obtain a sheet-like foam.
- each raw material of the foamable composition is kneaded using a kneading machine such as a Banbury mixer or a pressure kneader, and then continuously extruded using an extruder, calender, conveyor belt casting, etc. to form a sheet.
- foamable compositions can be produced.
- the ionizing radiation used in step (2) includes ⁇ rays, ⁇ rays, ⁇ rays, electron beams, etc., but electron beams are preferable.
- the irradiation amount of ionizing radiation may be sufficient as long as it can obtain the desired degree of crosslinking, but is preferably from 0.1 to 10 Mrad, more preferably from 0.2 to 5 Mrad, and even more preferably from 0.5 to 3 Mrad.
- the temperature at which the foamable composition is heated and foamed depends on the decomposition temperature of the thermally decomposable foaming agent used as the foaming agent, but is usually 140 to 300°C, preferably 150 to 280°C.
- step (3) it is preferable that the foam is stretched in one or both of MD and TD after foaming or while foaming. Moreover, after step (1), step (3) may be performed without passing through step (2). That is, the sheet-like foamable composition may be foamed without crosslinking.
- the molded article of the present invention is obtained by molding the polyolefin resin foam of the present invention.
- the molded article of the present invention can be obtained by molding the polyolefin resin foam of the present invention by a known method.
- other materials such as a base material and a skin material may be laminated and bonded to the polyolefin resin foam.
- the molded article of the present invention preferably has a skin material laminated on at least one surface of a polyolefin resin foam.
- Surface materials include polyvinyl chloride sheets, sheets made of a mixed resin of polyvinyl chloride and ABS resin, thermoplastic elastomer sheets, woven fabrics, knitted fabrics, non-woven fabrics, artificial leathers, and synthetic leathers using natural fibers and artificial fibers. Examples include leather and metal.
- the molded body may have a design such as a leather grain pattern or a wood grain pattern on the surface using genuine leather or a silicone stamper with irregularities transferred from stone, wood, or the like.
- Methods for bonding skin materials include, for example, extrusion lamination method, adhesive lamination method in which adhesive is applied and then laminated, thermal lamination method (thermal fusion method), hot melt method, high frequency welding method, electroless method for metals, etc.
- thermal lamination method thermal fusion method
- hot melt method hot melt method
- high frequency welding method high frequency welding method
- electroless method for metals etc.
- Examples include a plating method, an electrolytic plating method, and a vapor deposition method, but any method may be used as long as the two are bonded.
- Examples of methods for molding the molded article of the present invention include stamping molding, vacuum molding, compression molding, and injection molding. Among these, stamping molding method and vacuum molding method are preferred. As the vacuum forming method, both a male vacuum forming method and a female vacuum forming method can be employed, but the male vacuum forming method is more preferable.
- a molded article formed by molding the polyolefin resin foam of the present invention can be used as a heat insulating material, a cushioning material, and the like.
- the molded product formed by molding the polyolefin resin foam of the present invention does not easily generate odor even in the hot summer months, so it is used particularly in the automotive field for automotive interior materials such as ceiling materials, doors, and instrument panels. It can be suitably used as
- ⁇ Variation coefficient> A cross section of the polyolefin resin foam cut in the thickness direction along the TD direction was photographed at 200x magnification using a digital microscope (manufactured by Keyence Corporation, product name: VHX-900), and 50 pieces were taken. bubbles (cells) were observed. Then, each coefficient of variation was determined as follows.
- Bubble area (Pi) x (TD bubble diameter/2) x (ZD bubble diameter/2) Based on the 50 bubble areas thus determined, the average bubble area and the standard deviation of the bubble areas were determined. Then, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble area by the average bubble area was taken as the coefficient of variation of the bubble area.
- Coefficient of variation of bubble area Standard deviation of bubble area / Average bubble area
- ⁇ is the standard deviation
- X is the measurement data
- n is the number of measurements.
- ⁇ Crosslinking degree (gel fraction)> About 100 mg of a test piece was taken from the foam, and the mass A (mg) of the test piece was accurately weighed. Next, this test piece was immersed in 30 cm 3 of xylene at 115°C and left for 24 hours, filtered through a 200 mesh wire mesh to collect the insoluble matter on the wire mesh, vacuum dried, and the mass of the undissolved material was B (mg) was accurately weighed. From the obtained values, the degree of crosslinking (mass%) was calculated using the following formula. Gel fraction (mass%) 100 x (B/A)
- Heating dimensional change rates of MD and TD of the foam at 120°C were measured in accordance with JIS K 6767.
- ⁇ Odor evaluation> Two test pieces of 25 cm 3 (total 50 cm 3 ) were placed in a 1 L glass bottle, covered with a lid, and cured in an oven controlled at 105° C. for 2 hours. Then, the glass bottle was taken out and cooled to 23°C. I opened the lid of a glass bottle that had reached 23 degrees Celsius, brought my nose 1 cm from the mouth of the glass bottle, and smelled the odor. The odor grade was determined by comparing the intensity of the smelled odor to which level it corresponded to in the water diluted solution of n-butanol below.
- Odor grade 10 n-butanol concentration 0ml/L (pure water alone) Odor grade 9.0: n-butanol concentration 1.2ml/L Odor grade 8.0: n-butanol concentration 1.4ml/L Odor grade 7.0: n-butanol concentration 2.0ml/L Odor grade 6.0: n-butanol concentration 3.6ml/L Odor grade 5.5: n-butanol concentration 6.0ml/L Odor grade 5.0: n-butanol concentration 9.0ml/L Odor grade 4.5: n-butanol concentration 18.0ml/L Odor grade 4.0: n-butanol concentration 22.7ml/L Odor grade 3.0: n-butanol concentration 30.0ml/L Odor grade 2.0: n-butanol concentration 57.0ml/L Odor rating 1.0: n-butanol only
- the odor was evaluated by three people, and the evaluation was made based on the average value of the three people's odor ratings based on the following criteria.
- ⁇ Amount of filler in polyolefin resin foam The amount of filler relative to the total amount of polyolefin resin foam was measured by the following method. Put the polyolefin resin foam Xg (for example, 5 g) into a baking dish (heat-resistant temperature 1900°C, 150 mm x 150 mm x 5 mm), and place it in an electric muffle furnace (width 100 mm, depth 180 mm, height 100 mm, Yamato Scientific FM-27). I left it still. The temperature was raised from room temperature (25°C) to 200°C at a rate of 50°C/min in an air atmosphere and held for 30 minutes.
- Amount of filler in polyolefin resin foam [mass of combustion residue (g)/foam mass X (g)] x 100 Note that elemental analysis of the combustion residue can be performed using an ICP emission spectrometer mass spectrometer (SELFA SSGW-7602).
- Phenolic antioxidant Irganox 1010 (manufactured by BASF Japan), Tetrakis [methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane
- Phosphorous antioxidant Adekastab PEP- 8 (manufactured by ADEKA), 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane
- Example 1 Linear low-density polyethylene and magnesium oxide were put into an extruder, mixed, and cut into pellets to obtain a filler masterbatch having a magnesium oxide content of 20% by mass.
- the filler masterbatch, the polyolefin resin of the type listed in Table 1, a pyrolytic foaming agent, an antioxidant, and a crosslinking aid were put into an extruder and melt-kneaded to a thickness of 1.
- a foamable composition in the form of a sheet of .42 mm was obtained.
- the composition of the foamable composition is shown in Table 1. Both surfaces of the obtained sheet-like foamable composition were crosslinked by irradiating an electron beam of 2.0 Mrad at an accelerating voltage of 1000 kV.
- the obtained crosslinked foamable composition was heated to 270°C to obtain a foam having a density of 0.05 g/cm 3 (expansion ratio 20 cm 3 /g) and a thickness of 2.5 mm.
- Example 2 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 0.65 mm.
- the resulting foam had a density of 0.10 g/cm 3 (expansion ratio 10 cm 3 /g) and a thickness of 1.0 mm.
- Example 3 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.35 mm.
- the resulting foam had a density of 0.04 g/cm 3 (expansion ratio 25 cm 3 /g) and a thickness of 2.5 mm.
- Example 4 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.30 mm.
- the resulting foam had a density of 0.04 g/cm 3 (expansion ratio 25 cm 3 /g) and a thickness of 2.5 mm.
- Example 5 Random polypropylene and magnesium oxide were put into an extruder, mixed, and cut into pellets to obtain a filler masterbatch having a magnesium oxide content of 25% by mass.
- the filler masterbatch, the polyolefin resin of the type listed in Table 1, a pyrolytic foaming agent, an antioxidant, and a crosslinking aid were put into an extruder and melt-kneaded to a thickness of 1.
- a foamable composition in the form of a sheet of .85 mm was obtained.
- the composition of the foamable composition is shown in Table 1. Both surfaces of the obtained sheet-like foamable composition were crosslinked by irradiating an electron beam of 2.0 Mrad at an accelerating voltage of 1000 kV.
- the obtained crosslinked foamable composition was heated to 270°C to obtain a foam having a density of 0.05 g/cm 3 (expansion ratio 20 cm 3 /g) and a thickness of 3.6 mm.
- Example 6 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.45 mm.
- the resulting foam had a density of 0.07 g/cm 3 (expansion ratio 15 cm 3 /g) and a thickness of 2.0 mm.
- Example 7 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 0.85 mm.
- the resulting foam had a density of 0.05 g/cm 3 (expansion ratio 20 cm 3 /g) and a thickness of 1.5 mm.
- Example 8 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1. The resulting foam had a density of 0.05 g/cm 3 (expansion ratio 20 cm 3 /g) and a thickness of 2.5 mm.
- Example 9 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.45 mm.
- the resulting foam had a density of 0.07 g/cm 3 (expansion ratio 15 cm 3 /g) and a thickness of 2.0 mm.
- a polyolefin resin of the type listed in Table 1, a pyrolytic blowing agent, magnesium oxide, an antioxidant, and a crosslinking aid were put into an extruder and melt-kneaded to a thickness of 1.8 mm.
- a sheet-like foamable composition was obtained.
- the composition of the foamable composition is shown in Table 1. Both surfaces of the obtained sheet-like foamable composition were crosslinked by irradiating an electron beam of 2.0 Mrad at an accelerating voltage of 1000 kV.
- the obtained crosslinked foamable composition was heated to 270°C to obtain a foam having a density of 0.067 g/cm 3 (expansion ratio 15 cm 3 /g) and a thickness of 3.0 mm.
- Example 2 A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1. The resulting foam had a density of 0.05 g/cm 3 (expansion ratio 20 cm 3 /g) and a thickness of 2.5 mm.
- Comparative example 3 A foam was obtained in the same manner as in Comparative Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 0.65 mm.
- the resulting foam had a density of 0.10 g/cm 3 (expansion ratio 10 cm 3 /g) and a thickness of 1.0 mm.
- a foam was obtained in the same manner as in Comparative Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.30 mm.
- the resulting foam had a density of 0.04 g/cm 3 (expansion ratio 25 cm 3 /g) and a thickness of 2.0 mm.
- the foam of the present invention in which the metal oxide content is above a certain level and the coefficients of variation of TD cell diameter, ZD cell diameter, cell flatness, and cell area are below certain values, can reduce odor generation. I understand. On the other hand, it was found that the foam of Comparative Example 1, which had a large coefficient of variation, and the foams of Comparative Examples 2 to 4, which contained little or no metal oxide, generated a lot of odor.
Landscapes
- Chemical & Material Sciences (AREA)
- General Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Manufacture Of Porous Articles, And Recovery And Treatment Of Waste Products (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202380023891.XA CN118765301A (zh) | 2022-03-31 | 2023-03-31 | 聚烯烃系树脂发泡体及成型体 |
| JP2023523557A JP7875178B2 (ja) | 2022-03-31 | 2023-03-31 | ポリオレフィン系樹脂発泡体及び成形体 |
Applications Claiming Priority (4)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022060401 | 2022-03-31 | ||
| JP2022-060401 | 2022-03-31 | ||
| JP2022-143191 | 2022-09-08 | ||
| JP2022143191 | 2022-09-08 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023191081A1 true WO2023191081A1 (ja) | 2023-10-05 |
Family
ID=88202434
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/013652 Ceased WO2023191081A1 (ja) | 2022-03-31 | 2023-03-31 | ポリオレフィン系樹脂発泡体及び成形体 |
Country Status (2)
| Country | Link |
|---|---|
| JP (1) | JP7875178B2 (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023191081A1 (cg-RX-API-DMAC7.html) |
Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH01263130A (ja) * | 1988-04-14 | 1989-10-19 | Nippon Kiyouiku Sozai Kk | ポリエチレン系樹脂発泡体及びその製造方法並びに前記ポリエチレン系樹脂発泡体を用いてなる積木 |
| JPH06322167A (ja) * | 1993-05-11 | 1994-11-22 | Sekisui Chem Co Ltd | ポリオレフィン系樹脂発泡体の製造方法 |
| JP2002001829A (ja) * | 2000-06-16 | 2002-01-08 | Shinei Techno Kk | 複合発泡体の製造方法 |
| JP2013159753A (ja) * | 2012-02-08 | 2013-08-19 | Jsr Corp | 熱可塑性エラストマー組成物及び発泡成形体 |
| JP2018053226A (ja) * | 2016-09-30 | 2018-04-05 | 積水化学工業株式会社 | 架橋ポリオレフィン系樹脂発泡体 |
| JP2020172641A (ja) * | 2019-04-10 | 2020-10-22 | 日東電工株式会社 | 難燃発泡体および発泡部材 |
Family Cites Families (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4607059A (en) * | 1985-09-25 | 1986-08-19 | Pennwalt Corporation | Gas-releasing composition for tailoring gas evolution of system IR 2811 |
| JP7063566B2 (ja) * | 2017-09-29 | 2022-05-09 | 積水化学工業株式会社 | 樹脂発泡シート、樹脂発泡シートの製造方法、及び粘着テープ |
| JP7377047B2 (ja) * | 2019-09-27 | 2023-11-09 | 積水化学工業株式会社 | ポリオレフィン系樹脂発泡体シート、及びその製造方法 |
| CN112778565B (zh) * | 2020-12-30 | 2023-03-31 | 广德祥源新材科技有限公司 | 一种耐冲击的超薄型聚烯烃发泡片材及其制备方法和应用 |
-
2023
- 2023-03-31 JP JP2023523557A patent/JP7875178B2/ja active Active
- 2023-03-31 WO PCT/JP2023/013652 patent/WO2023191081A1/ja not_active Ceased
Patent Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH01263130A (ja) * | 1988-04-14 | 1989-10-19 | Nippon Kiyouiku Sozai Kk | ポリエチレン系樹脂発泡体及びその製造方法並びに前記ポリエチレン系樹脂発泡体を用いてなる積木 |
| JPH06322167A (ja) * | 1993-05-11 | 1994-11-22 | Sekisui Chem Co Ltd | ポリオレフィン系樹脂発泡体の製造方法 |
| JP2002001829A (ja) * | 2000-06-16 | 2002-01-08 | Shinei Techno Kk | 複合発泡体の製造方法 |
| JP2013159753A (ja) * | 2012-02-08 | 2013-08-19 | Jsr Corp | 熱可塑性エラストマー組成物及び発泡成形体 |
| JP2018053226A (ja) * | 2016-09-30 | 2018-04-05 | 積水化学工業株式会社 | 架橋ポリオレフィン系樹脂発泡体 |
| JP2020172641A (ja) * | 2019-04-10 | 2020-10-22 | 日東電工株式会社 | 難燃発泡体および発泡部材 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7875178B2 (ja) | 2026-06-17 |
| JPWO2023191081A1 (cg-RX-API-DMAC7.html) | 2023-10-05 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| CN108884257B (zh) | 交联聚烯烃系树脂发泡体及使用其的成型体 | |
| JP6698517B2 (ja) | 架橋ポリオレフィン系発泡体 | |
| CN107406612B (zh) | 交联聚烯烃系树脂发泡体 | |
| CN109790314B (zh) | 交联聚烯烃发泡体及使用了该交联聚烯烃发泡体的成型体 | |
| JP7377047B2 (ja) | ポリオレフィン系樹脂発泡体シート、及びその製造方法 | |
| JPWO2016039400A1 (ja) | 発泡体、積層体及び成形体 | |
| WO2021201056A1 (ja) | ポリオレフィン系樹脂発泡体シート及び車輌用内装材 | |
| JP5017740B2 (ja) | ポリオレフィン系樹脂架橋発泡体及びその製造方法 | |
| WO2018182034A1 (ja) | 発泡体及び成形体 | |
| JP2015145459A (ja) | 発泡体 | |
| JP7160615B2 (ja) | 架橋ポリオレフィン系樹脂発泡体 | |
| JPH02255738A (ja) | 部分架橋熱可塑性エラストマー発泡体およびその製造方法 | |
| US11680145B2 (en) | Crosslinked polyolefin foam and molded body using same | |
| CN118765301A (zh) | 聚烯烃系树脂发泡体及成型体 | |
| JP2021046506A (ja) | 発泡体シート | |
| JP7563930B2 (ja) | 発泡体及び車両用内装材 | |
| JP7518656B2 (ja) | 架橋ポリオレフィン系樹脂発泡体及び成形体 | |
| JP2023166277A (ja) | ポリオレフィン系架橋発泡体 | |
| JP2004182897A (ja) | 架橋ポリオレフィン系樹脂発泡体 | |
| JP2983304B2 (ja) | ポリオレフィン系樹脂架橋発泡体 | |
| CN121399198A (zh) | 复合体 | |
| JPH0649257A (ja) | ポリプロピレン架橋発泡体用樹脂組成物 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023523557 Country of ref document: JP |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23781089 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202380023891.X Country of ref document: CN |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 23781089 Country of ref document: EP Kind code of ref document: A1 |