WO2023063266A1 - 樹脂組成物 - Google Patents

樹脂組成物 Download PDF

Info

Publication number
WO2023063266A1
WO2023063266A1 PCT/JP2022/037690 JP2022037690W WO2023063266A1 WO 2023063266 A1 WO2023063266 A1 WO 2023063266A1 JP 2022037690 W JP2022037690 W JP 2022037690W WO 2023063266 A1 WO2023063266 A1 WO 2023063266A1
Authority
WO
WIPO (PCT)
Prior art keywords
resin composition
resin
mass
manufactured
group
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/037690
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
嘉生 西村
二朗 長岡
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ajinomoto Co Inc
Original Assignee
Ajinomoto Co Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ajinomoto Co Inc filed Critical Ajinomoto Co Inc
Priority to JP2023554505A priority Critical patent/JPWO2023063266A1/ja
Priority to CN202280068015.4A priority patent/CN118076697A/zh
Priority to KR1020247011930A priority patent/KR20240087832A/ko
Publication of WO2023063266A1 publication Critical patent/WO2023063266A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L63/00—Compositions of epoxy resins; Compositions of derivatives of epoxy resins
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B15/00—Layered products comprising a layer of metal
    • B32B15/04—Layered products comprising a layer of metal comprising metal as the main or only constituent of a layer, which is next to another layer of the same or of a different material
    • B32B15/08—Layered products comprising a layer of metal comprising metal as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B15/00—Layered products comprising a layer of metal
    • B32B15/04—Layered products comprising a layer of metal comprising metal as the main or only constituent of a layer, which is next to another layer of the same or of a different material
    • B32B15/08—Layered products comprising a layer of metal comprising metal as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin
    • B32B15/092—Layered products comprising a layer of metal comprising metal as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin comprising epoxy resins
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/18—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing
    • C08G59/40—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing characterised by the curing agents used
    • C08G59/4007—Curing agents not provided for by the groups C08G59/42 - C08G59/66
    • C08G59/4014—Nitrogen containing compounds
    • C08G59/4042—Imines; Imides
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/18—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing
    • C08G59/40—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing characterised by the curing agents used
    • C08G59/42—Polycarboxylic acids; Anhydrides, halides or low molecular weight esters thereof
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/18—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing
    • C08G59/40—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing characterised by the curing agents used
    • C08G59/62—Alcohols or phenols
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/18—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing
    • C08G59/40—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing characterised by the curing agents used
    • C08G59/62—Alcohols or phenols
    • C08G59/621—Phenols
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/01—Use of inorganic substances as compounding ingredients characterized by their specific function
    • C08K3/013—Fillers, pigments or reinforcing additives
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L101/00—Compositions of unspecified macromolecular compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L79/00—Compositions of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing nitrogen with or without oxygen or carbon only, not provided for in groups C08L61/00 - C08L77/00
    • C08L79/04—Polycondensates having nitrogen-containing heterocyclic rings in the main chain; Polyhydrazides; Polyamide acids or similar polyimide precursors
    • C08L79/08—Polyimides; Polyester-imides; Polyamide-imides; Polyamide acids or similar polyimide precursors
    • C08L79/085—Unsaturated polyimide precursors
    • H—ELECTRICITY
    • H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
    • H05K—PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
    • H05K1/00—Printed circuits
    • H05K1/02—Details
    • H05K1/03—Use of materials for the substrate
    • H—ELECTRICITY
    • H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
    • H05K—PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
    • H05K1/00—Printed circuits
    • H05K1/02—Details
    • H05K1/03—Use of materials for the substrate
    • H05K1/0313—Organic insulating material
    • H05K1/0353—Organic insulating material consisting of two or more materials, e.g. two or more polymers, polymer + filler, + reinforcement
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W74/00—Encapsulations, e.g. protective coatings
    • H10W74/40—Encapsulations, e.g. protective coatings characterised by their materials
    • H10W74/47—Encapsulations, e.g. protective coatings characterised by their materials comprising organic materials, e.g. plastics or resins
    • H10W74/473—Encapsulations, e.g. protective coatings characterised by their materials comprising organic materials, e.g. plastics or resins containing a filler

Definitions

  • the present invention relates to resin compositions.
  • the insulating layer is generally formed from a cured product obtained by curing a resin composition (Patent Document 1).
  • the cured product contained in the insulating layer is required to have a low dielectric loss tangent.
  • One of the methods for obtaining a cured product with a low dielectric loss tangent is to mix an active ester compound and an inorganic filler at a high concentration in a resin composition.
  • a resin composition containing a high concentration of an active ester compound and an inorganic filler is used, cracks tend to occur in the cured product, and the elongation at break of the cured product tends to decrease. there were.
  • the present invention has been invented in view of the above problems, a resin composition that has a low dielectric loss tangent, can suppress cracking, and can obtain a cured product with a large elongation at break; A cured product; a sheet-like laminate material containing the resin composition; a resin sheet having a resin composition layer formed from the resin composition; a printed wiring board provided with an insulating layer containing a cured product of the resin composition; , a semiconductor device comprising the printed wiring board;
  • the present inventors have made extensive studies to solve the above problems. As a result, the present inventors have found a resin containing (A) a biphenylaralkyl-type phenolic resin, (B) an epoxy resin, a specific range of amount of (C) an active ester compound, and a specific range of amount of (D) an inorganic filler.
  • the inventors have found that the composition can solve the above-mentioned problems, and completed the present invention. That is, the present invention includes the following.
  • a resin composition containing (A) a biphenyl aralkyl-type phenol resin, (B) an epoxy resin, (C) an active ester compound, and (D) an inorganic filler, (C) the amount of the active ester compound is 10% by mass or more with respect to 100% by mass of the non-volatile components of the resin composition; (D) The amount of the inorganic filler is 60% by mass or more with respect to 100% by mass of the nonvolatile components of the resin composition, or 45% by volume or more with respect to 100% by volume of the nonvolatile components of the resin composition. , resin composition.
  • each R h1 independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent
  • each R h2 independently represents an oxygen atom
  • R h3 each independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent
  • R h4 each independently has a substituent.
  • each Rh5 independently represents an alkyl group having 5 or more carbon atoms.
  • n h2 represents an integer of 0 to 10
  • m h each independently represents an integer of 0 to 4.
  • a resin sheet comprising a support and a resin composition layer formed on the support from the resin composition according to any one of [1] to [11].
  • a printed wiring board comprising an insulating layer containing a cured product of the resin composition according to any one of [1] to [11].
  • a semiconductor device comprising the printed wiring board according to [15].
  • a resin composition having a low dielectric loss tangent, capable of suppressing cracking, and capable of obtaining a cured product having a large elongation at break; a cured product of the resin composition; A sheet-like laminate material; a resin sheet having a resin composition layer formed from the resin composition; a printed wiring board having an insulating layer containing a cured product of the resin composition; and a semiconductor device having the printed wiring board; can provide
  • the resin composition according to one embodiment of the present invention includes (A) a biphenyl aralkyl-type phenol resin, (B) an epoxy resin, a specific range of amount of (C) an active ester compound, and a specific range of amount of (D) Inorganic fillers are included in combination.
  • this resin composition it is possible to obtain a cured product that has a low dielectric loss tangent, can suppress cracking, and has a high elongation at break.
  • This cured product is suitable, for example, as a material for insulating layers of printed wiring boards.
  • the resin composition according to the present embodiment contains (A) a biphenylaralkyl-type phenol resin as component (A).
  • the biphenylaralkyl-type phenolic resin contains a combination of a biphenylaralkyl structure and a phenolic structure in the molecule, and usually exhibits the function of curing the resin composition by reacting with the (B) epoxy resin.
  • this (A) biphenyl aralkyl-type phenolic resin is used in combination with components (B) to (D) as described above, a cured product having a low dielectric loss tangent, capable of suppressing cracking, and having a high elongation at break can be obtained. be able to.
  • a biphenyl aralkyl structure represents a structure in which a portion of the carbon chain, excluding both ends of an alkylene chain, is substituted with a biphenyl skeleton.
  • One or more substituents may be bonded to the biphenyl skeleton as long as the effects of the present invention are not significantly impaired. Examples of substituents include hydrocarbon groups such as alkyl groups and aryl groups.
  • a phenol structure represents a structure in which a hydroxyl group is bonded to a benzene ring.
  • One or more substituents may be bonded to the benzene ring of the phenol structure as long as the effects of the present invention are not significantly impaired.
  • substituents include hydrocarbon groups such as alkyl groups and aryl groups.
  • Preferred (A) biphenyl aralkyl-type phenolic resins include, for example, compounds represented by the following formula (A-1).
  • each R 1 independently represents an alkylene group
  • each R 2 independently represents a monovalent hydrocarbon group
  • each R 3 independently represents a monovalent represents a hydrocarbon group
  • n represents an integer of 1 to 20
  • s independently represents an integer of 0 to 4
  • t independently represents an integer of 0 to 3.
  • each R 1 independently represents an alkylene group.
  • the alkylene group may be linear or branched.
  • the number of carbon atoms in the alkylene group is preferably 1-10, more preferably 1-8, particularly preferably 1-5.
  • Examples of the alkylene group include methylene group, ethylene group, propylene group and the like.
  • each R 2 independently represents a monovalent hydrocarbon group.
  • the monovalent hydrocarbon group may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group.
  • the monovalent hydrocarbon group may be a linear or branched hydrocarbon group, or may be a hydrocarbon group containing a ring.
  • the monovalent hydrocarbon group preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and particularly preferably 1 to 6 carbon atoms.
  • Examples of monovalent hydrocarbon groups include alkyl groups such as methyl group, ethyl group, propyl group and butyl group; aryl groups such as phenyl group and naphthyl group;
  • each R 3 independently represents a monovalent hydrocarbon group.
  • the range of R 3 may be the same as R 2 above.
  • n represents an integer of 1-20. n is preferably 1-10, more preferably 1-6.
  • each s independently represents an integer of 0 to 4. s is preferably 0 or 1, particularly preferably 0.
  • each t independently represents an integer of 0 to 3.
  • t is preferably 0 or 1, particularly preferably 0.
  • the biphenylaralkyl-type phenolic resin is preferably a compound represented by the following formula (A-2).
  • R 4 each independently represents an alkyl group having 1 to 5 carbon atoms or a phenyl group, m each independently represents an integer of 1 to 5, n1 represents an integer of 1 to 20, and each t1 independently represents 0 or 1.
  • each R 4 independently represents an alkyl group having 1 to 5 carbon atoms or a phenyl group.
  • alkyl groups include a methyl group and an ethyl group.
  • each m independently represents an integer of 1 to 5.
  • m is preferably 1 to 4, more preferably 1 to 3, particularly preferably 1.
  • each n1 independently represents an integer of 1-20. n1 can be the same as n in formula (A-1).
  • each t1 independently represents 0 or 1. t1 is preferably zero.
  • Examples of particularly preferred (A) biphenylaralkyl-type phenolic resins include compounds represented by the following formula (A-3).
  • n2 usually represents an integer of 1-20, preferably 1-6.
  • a commercially available product may be used as the biphenyl aralkyl-type phenol resin.
  • Commercially available (A) biphenylaralkyl-type phenol resins include, for example, Nippon Kayaku's "KAYAHARD GPH-65”, “KAYAHARD GPH-78", and "KAYAHARD GPH-103" (all of which have the above formula (A-3 ) and compounds represented by ).
  • the biphenyl aralkyl-type phenol resin may be used singly or in combination of two or more.
  • the hydroxyl equivalent of the biphenylaralkyl-type phenol resin is preferably 50 g/eq. ⁇ 500 g/eq. , more preferably 50 g/eq. ⁇ 400 g/eq. , more preferably 100 g/eq. ⁇ 300 g/eq. is.
  • the hydroxyl equivalent represents the mass of resin per equivalent of hydroxyl.
  • the number of hydroxyl groups in the biphenylaralkyl-type phenol resin (A) is preferably 0.01 or more, more preferably 0.02 or more, and still more preferably 0.05 or more. preferably 1.5 or less, more preferably 1.0 or less, more preferably 0.9 or less, and particularly preferably 0.8 or less.
  • “(A) the number of hydroxyl groups of the biphenylaralkyl-type phenolic resin” means the sum of all the values obtained by dividing the mass of the non-volatile component of the (A) biphenylaralkyl-type phenolic resin present in the resin composition by the hydroxyl equivalent.
  • “(B) the number of epoxy groups of the epoxy resin” represents the sum of all the values obtained by dividing the mass of the non-volatile component of the (B) epoxy resin present in the resin composition by the epoxy equivalent.
  • the weight ratio W A /W B of the weight W A of (A) the biphenylaralkyl-type phenol resin and the weight W B of the (B) epoxy resin in the resin composition is preferably within a specific range.
  • the mass ratio W A /W B is preferably 0.01 or more, more preferably 0.03 or more, particularly preferably 0.05 or more, preferably 1.0 or less, more preferably 0. 0.7 or less, particularly preferably 0.6 or less.
  • the mass ratio W A /W C of the mass W A of (A) the biphenylaralkyl-type phenol resin and the mass W C of the (C) active ester compound in the resin composition is preferably within a specific range.
  • the mass ratio W A /W C is preferably 0.01 or more, more preferably 0.02 or more, particularly preferably 0.03 or more, preferably 0.80 or less, more preferably 0. 0.50 or less, particularly preferably 0.40 or less.
  • the amount of (A) the biphenylaralkyl-type phenolic resin in the resin composition is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and particularly It is preferably 0.5% by mass or more, preferably 10% by mass or less, more preferably 6% by mass or less, and particularly preferably 5% by mass or less.
  • the amount of (A) the biphenylaralkyl-type phenolic resin in the resin composition is preferably 0.1% by mass or more, more preferably 1% by mass or more, and particularly preferably 100% by mass of the resin component of the resin composition. It is 2% by mass or more, preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 15% by mass or less.
  • the resin component of the resin composition represents the non-volatile components of the resin composition excluding (D) the inorganic filler.
  • the resin composition according to the present embodiment contains (B) an epoxy resin as the (B) component.
  • the epoxy resin may be a curable resin having an epoxy group. Epoxy resin (B) does not include those corresponding to component (A) described above.
  • Epoxy resins include, for example, bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, and trisphenol type epoxy resins.
  • the epoxy resin preferably contains an epoxy resin containing an aromatic structure from the viewpoint of obtaining a cured product with excellent heat resistance.
  • Aromatic structures are chemical structures generally defined as aromatic and also include polycyclic aromatic and heteroaromatic rings.
  • Examples of epoxy resins containing an aromatic structure include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, Naphthol novolak type epoxy resin, phenol novolak type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, bixylenol type epoxy resin, glycidylamine type epoxy having an aromatic structure Resin, glycidyl ester type epoxy resin having aromatic structure, cresol novolak type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin having aromatic structure, epoxy resin having butad
  • the resin composition preferably contains an epoxy resin having two or more epoxy groups in one molecule as (B) the epoxy resin.
  • the ratio of the epoxy resin having two or more epoxy groups in one molecule to 100% by mass of the non-volatile components of the epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably is 70% by mass or more.
  • Epoxy resins include liquid epoxy resins at a temperature of 20° C. (hereinafter sometimes referred to as “liquid epoxy resins”) and solid epoxy resins at a temperature of 20° C. (hereinafter sometimes referred to as “solid epoxy resins”). ).
  • the resin composition may contain only a liquid epoxy resin, may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin. good.
  • a liquid epoxy resin having two or more epoxy groups in one molecule is preferable as the liquid epoxy resin.
  • liquid epoxy resins examples include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolak type epoxy resin, ester skeleton.
  • An alicyclic epoxy resin, a cyclohexane type epoxy resin, a cyclohexanedimethanol type epoxy resin, and an epoxy resin having a butadiene structure are preferred.
  • liquid epoxy resins include “HP4032”, “HP4032D”, and “HP4032SS” (naphthalene type epoxy resins) manufactured by DIC; “828US”, “828EL”, “jER828EL”, and “825" manufactured by Mitsubishi Chemical Corporation; “, “Epikote 828EL” (bisphenol A type epoxy resin); “jER807” and “1750” (bisphenol F type epoxy resin) manufactured by Mitsubishi Chemical Corporation; “jER152” (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; “630", “630LSD”, “604" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation; “ED-523T” (glycirrol type epoxy resin) manufactured by ADEKA; “EP-3950L” manufactured by ADEKA; “EP-3980S” (glycidylamine type epoxy resin); “EP-4088S” (dicyclopentadiene type epoxy resin) manufactured by ADEKA; Bisphenol F type epoxy resin mixture); “EX-721” (glycerol
  • the solid epoxy resin is preferably a solid epoxy resin having 3 or more epoxy groups per molecule, more preferably an aromatic solid epoxy resin having 3 or more epoxy groups per molecule.
  • Solid epoxy resins include bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, naphthol novolak type epoxy resin, cresol novolak type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, Naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, phenol aralkyl type epoxy resin, tetraphenylethane type epoxy resin, phenol phthalate A mijin-type epoxy resin is preferred.
  • solid epoxy resins include “HP4032H” (naphthalene-type epoxy resin) manufactured by DIC; “HP-4700” and “HP-4710” (naphthalene-type tetrafunctional epoxy resin) manufactured by DIC; “N-690” (cresol novolac type epoxy resin) manufactured by DIC Corporation; “N-695" (cresol novolak type epoxy resin) manufactured by DIC Corporation; "HP-7200”, “HP-7200HH”, “HP -7200H”, “HP-7200L” (dicyclopentadiene type epoxy resin); DIC's "EXA-7311", “EXA-7311-G3", “EXA-7311-G4", “EXA-7311-G4S” ", "HP6000” (naphthylene ether type epoxy resin); Nippon Kayaku "EPPN-502H” (trisphenol type epoxy resin); Nippon Kayaku “NC7000L” (naphthol novolac type epoxy resin); "NC3
  • the epoxy equivalent of the epoxy resin is preferably 50 g/eq. ⁇ 5,000 g/eq. , more preferably 60 g/eq. ⁇ 3,000 g/eq. , more preferably 80 g/eq. ⁇ 2,000 g/eq. , particularly preferably 110 g/eq. ⁇ 1,000g/eq. is.
  • Epoxy equivalent weight represents the mass of resin per equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.
  • the weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, still more preferably 400 to 1,500.
  • the weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by a gel permeation chromatography (GPC) method.
  • the amount of (B) the epoxy resin in the resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, and particularly preferably 4% by mass or more, relative to 100% by mass of the non-volatile components in the resin composition. , preferably 25% by mass or less, more preferably 20% by mass or less, and particularly preferably 10% by mass or less.
  • the amount of (B) epoxy resin is within the above range, effects such as reduction in dielectric loss tangent of the cured product of the resin composition, suppression of cracking, and increase in elongation at break can be obtained remarkably.
  • the amount of (B) epoxy resin in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 20% by mass or more, relative to 100% by mass of the resin component in the resin composition. , preferably 60% by mass or less, more preferably 50% by mass or less, and particularly preferably 40% by mass or less.
  • amounts of (B) epoxy resin is within the above range, effects such as reduction in dielectric loss tangent of the cured product of the resin composition, suppression of cracking, and increase in elongation at break can be obtained remarkably.
  • the resin composition according to the present embodiment contains the (C) active ester compound as the (C) component in a content within a specific range.
  • (C) Active ester compounds do not include those corresponding to the above components (A) and (B).
  • the active ester compound can function as an epoxy resin curing agent that reacts with the (B) epoxy resin to cure the resin composition.
  • (C) Active ester compounds may be used singly or in combination of two or more.
  • the active ester compound generally contains two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds. is preferably used.
  • the active ester compound is preferably obtained by a condensation reaction between a carboxylic acid compound and/or a thiocarboxylic acid compound and a hydroxy compound and/or a thiol compound.
  • an active ester compound obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester compound obtained from a carboxylic acid compound and a phenol compound and/or a naphthol compound is more preferred.
  • carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.
  • phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalin, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m- cresol, p-cresol, catechol, ⁇ -naphthol, ⁇ -naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucine, Benzenetriol, dicyclopentadiene-type diphenol compound, phenol no
  • the (C) active ester compound includes a dicyclopentadiene-type active ester compound, a naphthalene-type active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, and a benzoylated product of phenol novolak.
  • Active ester compounds are preferred, among which at least one selected from dicyclopentadiene-type active ester compounds and naphthalene-type active ester compounds is more preferred, and naphthalene-type active ester compounds are particularly preferred.
  • an active ester compound containing a dicyclopentadiene-type diphenol structure is preferable. Further, as one aspect of the present invention, it preferably contains a dicyclopentadiene-type active ester compound and a naphthalene-type active ester compound.
  • active ester compounds include, for example, "EXB9451”, “EXB9460”, “EXB9460S”, “EXB-8000L” and “EXB-8000L” as active ester compounds containing a dicyclopentadiene type diphenol structure.
  • the active ester group equivalent of the active ester compound is preferably 50 g/eq. ⁇ 500 g/eq. , more preferably 50 g/eq. ⁇ 400 g/eq. , more preferably 100 g/eq. ⁇ 300 g/eq. is.
  • the active ester group equivalent represents the mass of the active ester compound per equivalent of active ester group.
  • the number of active ester groups in the active ester compound (C) is preferably 0.1 or more, more preferably 0.5 or more, and still more preferably 0.8 or more. , preferably 6.0 or less, more preferably 5.0 or less, and particularly preferably 4.0 or less.
  • (C) active ester group number of the active ester compound refers to the sum of all the values obtained by dividing the mass of the non-volatile components of the active ester compound (C) present in the resin composition by the active ester group equivalent.
  • the number of active ester groups in (C) the active ester compound is preferably 1.0 or more, more preferably 1.5 or more, and particularly preferably 2.0. or more, preferably 50 or less, more preferably 40 or less, and particularly preferably 30 or less.
  • the amount of (C) the active ester compound in the resin composition is usually 10% by mass or more, preferably 11% by mass or more, and particularly preferably 12% by mass or more, relative to 100% by mass of the non-volatile components of the resin composition. , preferably 30% by mass or less, more preferably 25% by mass or less, and particularly preferably 20% by mass or less.
  • the amount of the active ester compound is within the above range, the dielectric loss tangent of the cured product of the resin composition can be reduced, cracking can be suppressed, and the elongation at break can be increased.
  • the amount of (C) the active ester compound in the resin composition is preferably 20% by mass or more, more preferably 30% by mass or more, and particularly preferably 40% by mass or more, relative to 100% by mass of the resin component of the resin composition. , preferably 80% by mass or less, more preferably 70% by mass or less, and particularly preferably 60% by mass or less.
  • the amount of (C) the active ester compound is within the above range, the effects of reducing the dielectric loss tangent of the cured product of the resin composition, suppressing cracking, and increasing the elongation at break can be remarkably obtained.
  • the resin composition according to the present embodiment contains the inorganic filler (D) as the component (D) in a content within a specific range.
  • the inorganic filler is usually contained in the resin composition in the form of particles.
  • An inorganic compound is used as the material for the inorganic filler.
  • inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, and water.
  • an inorganic composite oxide may be used as the material for (D) the inorganic filler.
  • An inorganic complex oxide represents an oxide containing two or more kinds of atoms selected from the group consisting of metal atoms and metalloid atoms.
  • Such an inorganic composite oxide is preferably an oxide containing a combination of silicon and one or more atoms selected from the group consisting of metal atoms other than silicon and metalloid atoms.
  • Metal atoms to be combined with silicon include aluminum, lead, nickel, cobalt, copper, zinc, zirconium, iron, lithium, magnesium, barium, potassium, calcium, titanium, boron, sodium, etc. Among them, aluminum is particularly preferred. . Therefore, as the inorganic composite oxide, an oxide containing silicon and aluminum is preferable, and an aluminosilicate is particularly preferable.
  • silica silica, alumina and aluminosilicate are preferred, and silica is particularly preferred.
  • examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica.
  • silica spherical silica is preferable.
  • the inorganic filler may be used singly or in combination of two or more.
  • Inorganic fillers can be classified into hollow inorganic fillers having internal voids and solid inorganic fillers having no internal voids.
  • As the inorganic filler only a hollow inorganic filler may be used, only a solid inorganic filler may be used, or a combination of a hollow inorganic filler and a solid inorganic filler may be used. . When hollow inorganic fillers are used, the dielectric constant of the cured resin composition can usually be lowered.
  • the hollow inorganic filler Since the hollow inorganic filler has pores, it usually has a porosity greater than 0% by volume. From the viewpoint of lowering the dielectric constant of the insulating layer containing the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 10% by volume or more, more preferably 15% by volume or more, and particularly preferably 20% by volume. % or more. Further, from the viewpoint of the mechanical strength of the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 95% by volume or less, more preferably 90% by volume or less, and particularly preferably 85% by volume or less. .
  • the porosity P (% by volume) of a particle is the volume-based ratio of the total volume of one or more pores present inside the particle to the volume of the entire particle based on the outer surface of the particle (total volume of pores /particle volume).
  • the porosity P is obtained by using the measured value D M (g/cm 3 ) of the actual density of the particles and the theoretical value D T (g/cm 3 ) of the substance density of the material forming the particles. It can be calculated by the formula (X1).
  • the manufacturing method of the hollow inorganic filler is not particularly limited, and it can be manufactured by a conventional method.
  • inorganic fillers include, for example, "SP60-05” and “SP507-05” manufactured by Nippon Steel & Sumikin Materials; “YC100C”, “YA050C” and “YA050C-MJE” manufactured by Admatechs.
  • the average particle diameter of the inorganic filler is preferably 0.01 ⁇ m or more, more preferably 0.05 ⁇ m or more, still more preferably 0.1 ⁇ m or more, and particularly preferably from the viewpoint of significantly obtaining the desired effects of the present invention. is 0.2 ⁇ m or more, preferably 10 ⁇ m or less, more preferably 5 ⁇ m or less, still more preferably 3 ⁇ m or less.
  • the average particle size of the inorganic filler can be measured by a laser diffraction/scattering method based on Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction/scattering type particle size distribution measuring device, and the median diameter can be used as the average particle size for measurement.
  • a measurement sample can be obtained by weighing 100 mg of an inorganic filler and 10 g of methyl ethyl ketone in a vial and dispersing them with ultrasonic waves for 10 minutes.
  • a measurement sample is measured using a laser diffraction particle size distribution measuring device, the wavelengths of the light source used are blue and red, the volume-based particle size distribution of the inorganic filler is measured by the flow cell method, and from the obtained particle size distribution
  • the average particle size can be calculated as the median size.
  • the laser diffraction particle size distribution analyzer include "LA-960" manufactured by Horiba, Ltd., and the like.
  • the specific surface area of the inorganic filler is preferably 0.1 m 2 /g or more, more preferably 0.5 m 2 /g or more, and still more preferably 1 m 2 from the viewpoint of significantly obtaining the desired effects of the present invention. /g or more, particularly preferably 3 m 2 /g or more, preferably 100 m 2 /g or less, more preferably 70 m 2 /g or less, even more preferably 50 m 2 /g or less, particularly preferably 40 m 2 /g or less. be.
  • the specific surface area of the inorganic filler is determined by adsorbing nitrogen gas on the sample surface using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech) according to the BET method, and calculating the specific surface area using the BET multipoint method. can be measured by
  • the inorganic filler is preferably treated with a surface treatment agent from the viewpoint of enhancing moisture resistance and dispersibility.
  • surface treatment agents include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate compounds.
  • a coupling agent etc. are mentioned.
  • One type of surface treatment agent may be used alone, or two or more types may be used in combination.
  • Examples of commercially available surface treatment agents include “KBM403” (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM803” (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., Shin-Etsu Chemical Industry Co., Ltd. "KBE903” (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd. "KBM573” (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.
  • the degree of surface treatment with a surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with a surface treatment agent of 0.2% to 5% by mass, and a surface treatment agent of 0.2% to 3% by mass. It is more preferably surface-treated, and more preferably surface-treated with 0.3% by mass to 2% by mass of a surface treating agent.
  • the degree of surface treatment by the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler.
  • the amount of carbon per unit surface area of the inorganic filler is preferably 0.02 mg/m 2 or more, more preferably 0.1 mg/m 2 or more, and more preferably 0.2 mg/m 2 from the viewpoint of improving the dispersibility of the inorganic filler. The above is more preferable.
  • it is preferably 1.0 mg/m 2 or less, more preferably 0.8 mg/m 2 or less, and even more preferably 0.5 mg/m 2 or less.
  • the amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (eg, methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler surface-treated with the surface treatment agent, and ultrasonic cleaning is performed at 25° C. for 5 minutes. After removing the supernatant liquid and drying the solid content, a carbon analyzer can be used to measure the amount of carbon per unit surface area of the inorganic filler. As a carbon analyzer, "EMIA-320V" manufactured by Horiba Ltd. can be used.
  • EMIA-320V manufactured by Horiba Ltd.
  • the amount of (D) the inorganic filler in the resin composition satisfies at least one of the following conditions (i) and (ii).
  • the amount (% by mass) of the inorganic filler is usually 60% by mass or more, preferably 63% by mass or more, more preferably 65% by mass or more, and particularly preferably 100% by mass of the non-volatile components of the resin composition. is 67% by mass or more, preferably 85% by mass or less, more preferably 80% by mass or less, and particularly preferably 75% by mass or less.
  • the amount (% by volume) of the inorganic filler is usually 45% by volume or more, preferably 50% by volume or more, more preferably 55% by volume or more with respect to 100% by volume of the non-volatile components of the resin composition,
  • the content is preferably 80% by volume or less, more preferably 70% by volume or less, and particularly preferably 65% by volume or less.
  • the resin composition according to the present embodiment may further contain (E) an optional curing agent as an optional component in combination with the above-described components (A) to (D).
  • the (E) optional curing agent as the (E) component does not include those corresponding to the above-described components (A) to (D).
  • the optional curing agent is the same as (A) the biphenyl aralkyl-type phenol resin and (C) the active ester compound described above, and (B) an epoxy resin curing agent that reacts with the epoxy resin to cure the resin composition. can have a function.
  • Any curing agent may be used singly or in combination of two or more.
  • optional curing agents examples include phenol-based curing agents, carbodiimide-based curing agents, acid anhydride-based curing agents, amine-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and thiol-based curing agents. agents.
  • phenol-based curing agents classified as optional curing agents do not include those corresponding to (A) biphenylaralkyl-type phenolic resins.
  • carbodiimide-based curing agent a curing agent having one or more, preferably two or more carbodiimide structures in one molecule can be used.
  • carbodiimide-based curing agents include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexanebis(methylene-t-butylcarbodiimide); biscarbodiimides such as biscarbodiimide; aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), Poly(naphthylenecarbodiimide), Poly(tolylenecarbodiimide), Poly(methyldiisopropylpheny
  • carbodiimide curing agents examples include “Carbodilite V-02B”, “Carbodilite V-03”, “Carbodilite V-04K”, “Carbodilite V-07” and “Carbodilite V-09” manufactured by Nisshinbo Chemical Co., Ltd. "Stabaxol P”, “Stabaxol P400”, and “Hykasil 510” manufactured by Rhein Chemie.
  • a curing agent having one or more, preferably two or more hydroxyl groups bonded to an aromatic ring such as a benzene ring or a naphthalene ring per molecule can be used.
  • a phenol-based curing agent having a novolac structure is preferred.
  • a nitrogen-containing phenolic curing agent is preferable, and a triazine skeleton-containing phenolic curing agent is more preferable.
  • a triazine skeleton-containing phenol novolak resin is preferable from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion.
  • phenol-based curing agent examples include, for example, "MEH-7700”, “MEH-7810", and “MEH-7851” manufactured by Meiwa Kasei Co., Ltd., “NHN” and “CBN” manufactured by Nippon Kayaku, Japan “SN-170”, “SN-180”, “SN-190”, “SN-475”, “SN-485”, “SN-495”, “SN-375”, “ SN-395”, DIC's "LA-7052", “LA-7054”, “LA-3018”, “LA-3018-50P", “LA-1356”, “TD2090”, “TD-2090- 60M” and the like.
  • acid anhydride-based curing agent a curing agent having one or more acid anhydride groups in one molecule can be used, and a curing agent having two or more acid anhydride groups in one molecule is used.
  • acid anhydride curing agents include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, and hydrogenated methylnadic acid.
  • Examples of commercially available acid anhydride curing agents include “HNA-100”, “MH-700”, “MTA-15”, “DDSA” and “OSA” manufactured by Shin Nippon Rika; “YH-306”, “YH-307” of Hitachi Chemical Co., Ltd. "HN-2200”, “HN-5500”; Clay Valley Co., Ltd. "EF-30”, “EF-40” “EF-60”, “EF-80” and the like.
  • amine-based curing agent a curing agent having one or more, preferably two or more amino groups in one molecule can be used.
  • amine-based curing agents include aliphatic amines, polyetheramines, alicyclic amines, aromatic amines, etc. Among them, aromatic amines are preferred.
  • Amine-based curing agents are preferably primary amines or secondary amines, more preferably primary amines.
  • Specific examples of amine curing agents include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, and 3,3'-diaminodiphenylsulfone.
  • amine-based curing agents examples include “SEIKACURE-S” manufactured by Seika; AB", “Kayahard AS”; “Epicure W” manufactured by Mitsubishi Chemical; “DTDA” manufactured by Sumitomo Seika.
  • benzoxazine-based curing agents include “JBZ-OP100D” and “ODA-BOZ” manufactured by JFE Chemical Co., Ltd.; “HFB2006M” manufactured by Showa Polymer Co., Ltd.; Examples include “Fa”.
  • cyanate ester curing agents include bisphenol A dicyanate, polyphenolcyanate (oligo(3-methylene-1,5-phenylenecyanate)), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4, 4′-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatophenylmethane), bis(4-cyanate-3,5- Difunctional cyanate resins such as dimethylphenyl)methane, 1,3-bis(4-cyanatophenyl-1-(methylethylidene))benzene, bis(4-cyanatophenyl)thioether, and bis(4-cyanatophenyl)ether, Polyfunctional cyanate resins derived from phenol novolak, cresol novolak, etc., and prepolymers obtained by partially triazine-forming these cyan
  • cyanate ester curing agents include “PT30” and “PT60” (both phenol novolac type polyfunctional cyanate ester resins), “BA230” and “BA230S75” (part of bisphenol A dicyanate) manufactured by Lonza Japan Co., Ltd. or a prepolymer that is entirely triazined to form a trimer), and the like.
  • thiol-based curing agents examples include trimethylolpropane tris (3-mercaptopropionate), pentaerythritol tetrakis (3-mercaptobutyrate), tris (3-mercaptopropyl) isocyanurate, and the like.
  • the active group equivalent of any curing agent is preferably 50 g/eq. ⁇ 3000g/eq. , more preferably 100 g/eq. ⁇ 1000 g/eq. , more preferably 100 g/eq. ⁇ 500 g/eq. , particularly preferably 100 g/eq. ⁇ 300 g/eq. is.
  • Active group equivalents represent the mass of curing agent per equivalent of active groups.
  • the amount of the optional curing agent (E) in the resin composition may be 0% by mass, may be greater than 0% by mass, and preferably 0% by mass with respect to 100% by mass of the non-volatile components of the resin composition. 0.01% by mass or more, more preferably 0.1% by mass or more, particularly preferably 1.0% by mass or more, preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less is.
  • the amount of (E) the optional curing agent in the resin composition may be 0% by mass, may be greater than 0% by mass, and preferably 0% by mass with respect to 100% by mass of the resin component of the resin composition. .1% by mass or more, more preferably 1.0% by mass or more, particularly preferably 5.0% by mass or more, preferably 50% by mass or less, more preferably 40% by mass or less, and particularly preferably 30% by mass or less is.
  • the resin composition according to the present embodiment may further contain (F) a curing accelerator as an optional component in combination with the components (A) to (E) described above.
  • the (F) curing accelerator as the (F) component does not include those corresponding to the above-described components (A) to (E).
  • the (F) curing accelerator functions as a curing catalyst that accelerates the curing of the (B) epoxy resin.
  • curing accelerators examples include phosphorus curing accelerators, urea curing accelerators, guanidine curing accelerators, imidazole curing accelerators, metal curing accelerators, and amine curing accelerators. . Among them, imidazole-based curing accelerators are preferred.
  • the curing accelerator may be used alone or in combination of two or more.
  • Phosphorus curing accelerators include, for example, tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium) pyromellitate, tetrabutylphosphonium hydro Aliphatic phosphonium salts such as genhexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, di-tert-butyldimethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltripheny
  • Urea-based curing accelerators include, for example, 1,1-dimethylurea; 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, 3- Aliphatic dimethylurea such as cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl )-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4- methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1,1-dimethylurea, 3-(4-isopropylphenyl)-1,1-dimethyl
  • Guanidine curing accelerators include, for example, dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, Tetramethylguanidine, Pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0] Dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1 -allylbiguanide, 1-phenylbiguanide, 1-(o-tolyl)biguanide and
  • imidazole curing accelerators examples include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl- 2-phenylimidazolium trimellitate, 2,4-d
  • imidazole curing accelerators include, for example, Shikoku Kasei Co., Ltd. "1B2PZ”, “2E4MZ”, “2MZA-PW”, “2MZ-OK”, “2MA-OK”, “2MA-OK- PW”, “2PHZ”, “2PHZ-PW”, "Cl1Z”, “Cl1Z-CN”, “Cl1Z-CNS”, “C11Z-A”; and "P200-H50” manufactured by Mitsubishi Chemical Corporation.
  • metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin.
  • organometallic complexes include organocobalt complexes such as cobalt (II) acetylacetonate and cobalt (III) acetylacetonate, organocopper complexes such as copper (II) acetylacetonate, and zinc (II) acetylacetonate.
  • organic zinc complexes such as iron (III) acetylacetonate; organic nickel complexes such as nickel (II) acetylacetonate; organic manganese complexes such as manganese (II) acetylacetonate;
  • organic metal salts include zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
  • amine curing accelerators examples include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo (5,4,0)-undecene and the like.
  • amine-based curing accelerator a commercially available product may be used, such as "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd., and the like.
  • the amount of the (F) curing accelerator in the resin composition may be 0% by mass, or may be greater than 0% by mass, preferably 0.0% by mass, relative to 100% by mass of non-volatile components in the resin composition. 01% by mass or more, more preferably 0.02% by mass or more, particularly preferably 0.03% by mass or more, preferably 1.0% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0 .1% by mass or less.
  • the amount of the (F) curing accelerator in the resin composition may be 0% by mass or greater than 0% by mass, preferably 0.0% by mass, relative to 100% by mass of the resin component of the resin composition. 01% by mass or more, more preferably 0.05% by mass or more, particularly preferably 0.1% by mass or more, preferably 2.0% by mass or less, more preferably 1.5% by mass or less, particularly preferably 1 0% by mass or less.
  • the resin composition according to the present embodiment may further contain (G) a thermoplastic resin as an optional component in combination with the components (A) to (F) described above.
  • the (G) thermoplastic resin as the (G) component does not include those corresponding to the above-described components (A) to (F).
  • Thermoplastic resins include, for example, phenoxy resins, polyimide resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyamideimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, and polycarbonate resins. , polyether ether ketone resin, polyester resin, and the like.
  • the thermoplastic resin may be used alone or in combination of two or more.
  • phenoxy resins include bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, and terpene.
  • Examples include phenoxy resins having one or more skeletons selected from the group consisting of skeletons and trimethylcyclohexane skeletons.
  • the terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
  • phenoxy resin examples include Mitsubishi Chemical's "1256” and “4250” (both bisphenol A skeleton-containing phenoxy resins); Mitsubishi Chemical's “YX8100” (bisphenol S skeleton-containing phenoxy resin); Mitsubishi Chemical "YX6954” (bisphenolacetophenone skeleton-containing phenoxy resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "FX280” and “FX293” manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "YL7769BH30", “YL6794", "YL7213", “YL7290”, “YL7482” and “YL7891BH30”;
  • polyimide resins include “SLK-6100” manufactured by Shin-Etsu Chemical Co., Ltd., and “Likacoat SN20” and “Ricacoat PN20” manufactured by Shin Nippon Rika.
  • polyvinyl acetal resins examples include polyvinyl formal resins and polyvinyl butyral resins, with polyvinyl butyral resins being preferred.
  • Specific examples of polyvinyl acetal resins include Denka Butyral 4000-2, Denka Butyral 5000-A, Denka Butyral 6000-C, and Denka Butyral 6000-EP manufactured by Sekisui Chemical Co., Ltd. S-LEC BH series, BX series (eg BX-5Z), KS series (eg KS-1), BL series, BM series;
  • polyolefin resins include ethylene-based copolymers such as low-density polyethylene, ultra-low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer.
  • Resin polyolefin polymers such as polypropylene and ethylene-propylene block copolymers.
  • polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxyl group-containing polybutadiene resins, phenolic hydroxyl group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, and isocyanate group-containing resins.
  • examples include polybutadiene resin, urethane group-containing polybutadiene resin, polyphenylene ether-polybutadiene resin, and the like.
  • polyamide-imide resins include “Vylomax HR11NN” and “Vylomax HR16NN” manufactured by Toyobo.
  • polyamideimide resins include modified polyamideimides such as “KS9100” and “KS9300” (polysiloxane skeleton-containing polyamideimides) manufactured by Hitachi Chemical Co., Ltd.
  • polyethersulfone resin examples include “PES5003P” manufactured by Sumitomo Chemical Co., Ltd.
  • polysulfone resins include polysulfone "P1700” and “P3500” manufactured by Solvay Advanced Polymers.
  • polyphenylene ether resin examples include "NORYL SA90” manufactured by SABIC.
  • polyetherimide resin examples include "Ultem” manufactured by GE.
  • polycarbonate resins examples include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxy group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins.
  • Specific examples of polycarbonate resins include "FPC0220” manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and “T6001” (polycarbonate diol) manufactured by Asahi Kasei Chemicals, “C-1090” and “C-2090” manufactured by Kuraray Co., Ltd. , “C-3090” (polycarbonate diol) and the like.
  • Specific examples of the polyetheretherketone resin include "Sumiproy K” manufactured by Sumitomo Chemical Co., Ltd., and the like.
  • polyester resins include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, polycyclohexanedimethyl terephthalate resin, and the like.
  • the weight average molecular weight (Mw) of the thermoplastic resin is preferably greater than 5,000, more preferably 8,000 or more, still more preferably 10,000 or more, particularly preferably 20,000 or more, and preferably is 100,000 or less, more preferably 70,000 or less, still more preferably 60,000 or less, and particularly preferably 50,000 or less.
  • the amount of the (G) thermoplastic resin in the resin composition may be 0% by mass, or may be greater than 0% by mass, preferably 0.0% by mass, relative to 100% by mass of non-volatile components in the resin composition. 01% by mass or more, more preferably 0.02% by mass or more, particularly preferably 0.03% by mass or more, preferably 1.0% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0 .1% by mass or less.
  • the amount of the (G) thermoplastic resin in the resin composition may be 0% by mass or greater than 0% by mass, preferably 0.0% by mass, relative to 100% by mass of the resin component of the resin composition. 01% by mass or more, more preferably 0.05% by mass or more, particularly preferably 0.1% by mass or more, preferably 2.0% by mass or less, more preferably 1.5% by mass or less, particularly preferably 1 0% by mass or less.
  • the resin composition according to the present embodiment may further contain (H) a maleimide resin as an optional component in combination with the components (A) to (G) described above.
  • the (H) maleimide resin as the (H) component does not include those corresponding to the above-described components (A) to (G).
  • As the maleimide resin compounds containing at least one, preferably two or more maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule can be used. .
  • Maleimide resins can be reacted with (B) epoxy resins in the presence of a suitable catalyst such as an imidazole compound.
  • (H) maleimide resin the ethylenic double bond contained in the maleimide group can cause radical polymerization. Therefore, the (H) maleimide resin can thermoset the resin composition by these reactions.
  • the maleimide resin When the maleimide resin is used, the dielectric loss tangent of the cured product of the resin composition can be particularly effectively reduced.
  • maleimide resin an aliphatic maleimide resin containing an aliphatic amine skeleton may be used, an aromatic maleimide resin containing an aromatic amine skeleton may be used, or a combination thereof may be used. Moreover, (H) maleimide resin may be used individually by 1 type, and may be used in combination of 2 or more types.
  • the maleimide resin is preferably one or more selected from the group consisting of a maleimide resin represented by the following formula (H-1) and a maleimide resin represented by the following formula (H-2).
  • each R h1 independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent
  • each R h2 independently represents an oxygen atom, represents an arylene group, an alkylene group, or a divalent group consisting of a combination of two or more of these groups, where n h1 represents an integer of 1-15
  • R h3 each independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent
  • R h4 each independently has a substituent.
  • each Rh5 independently represents an alkyl group having 5 or more carbon atoms.
  • n h2 represents an integer of 0 to 10
  • m h each independently represents an integer of 0 to 4.
  • Each R h1 independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent.
  • the number of carbon atoms in the divalent aliphatic group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, still more preferably 40 or less.
  • This divalent aliphatic group may be linear, branched or cyclic, with linear being preferred.
  • the cyclic aliphatic group is a concept that includes both a cyclic aliphatic group and a linear aliphatic group and a cyclic aliphatic group. Examples of divalent aliphatic groups include alkylene groups and alkenylene groups.
  • alkylene groups examples include pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, tridecylene, heptadecylene, hexatriacontylene, and octylene-cyclohexylene.
  • a group having a structure a group having an octylene-cyclohexylene-octylene structure, a group having a propylene-cyclohexylene-octylene structure, and the like, and a hexatriacontylene group is preferred.
  • alkenylene groups include pentynylene, hexynylene, heptylene, octinylene, nonynylene, decinylene, undecynylene, dodecynylene, tridecynylene, heptadecinylene, hexatriacontinylene, and octinylene-cyclohexynylene structures.
  • a group having an octinylene-cyclohexynylene-octinylene structure, a group having a propynylene-cyclohexynylene-octinylene structure, etc., and a hexatriacontinylene group is preferred.
  • Substituents for the divalent aliphatic group include, for example, a halogen atom, —OH, —O—C 1-10 alkyl group, —N(C 1-10 alkyl group) 2 , C 1-10 alkyl group, C 2-30 alkenyl group, C 2-30 alkynyl group, C 6-10 aryl group, —NH 2 , —CN, —C(O)O—C 1-10 alkyl group, —COOH, —C(O)H , -NO 2 and the like.
  • C xy (where x and y are positive integers and satisfies x ⁇ y) means that the organic group described immediately after this term has x to y carbon atoms. represents something.
  • C 1-10 alkyl group indicates an alkyl group having 1 to 10 carbon atoms.
  • substituents may combine with each other to form a ring, and the ring structure includes spiro rings and condensed rings.
  • the substituents are preferably alkyl groups having 5 or more carbon atoms.
  • Each R h2 independently represents an oxygen atom, an arylene group, an alkylene group, or a divalent group consisting of a combination of two or more of these groups.
  • R h2 is preferably a divalent group consisting of a combination of two or more of these groups or an oxygen atom.
  • a combination of an oxygen atom, an arylene group, and an alkylene group can be mentioned as a divalent group consisting of a combination of two or more of these groups.
  • Specific examples of the divalent group consisting of a combination of two or more of these groups include the following groups. In the formula, "*" represents a bond.
  • n h1 represents an integer of 1-15, preferably an integer of 1-10.
  • Each R h3 independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent.
  • R h3 is the same divalent aliphatic group having 5 or more carbon atoms which may have a substituent represented by R h1 , and a hexylene group, a heptylene group, an octylene group, a nonylene group and a decylene group are An octylene group is preferred, and an octylene group is more preferred.
  • R h4 independently represents a divalent group having an optionally substituted aromatic ring.
  • R h4 is a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; a group consisting of a combination of a divalent group derived from phthalimide and an alkylene group is preferable; A group consisting of a combination of divalent groups is more preferred.
  • R h4 Specific examples of the group represented by R h4 include the following groups.
  • "*" represents a bond.
  • Each R h5 independently represents an alkyl group having 5 or more carbon atoms.
  • the number of carbon atoms in the alkyl group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, still more preferably 40 or less.
  • This alkyl group may be linear, branched, or cyclic, with linear being preferred. Examples of such alkyl groups include pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups.
  • An alkyl group having 5 or more carbon atoms may be substituted for an alkylene group having 5 or more carbon atoms.
  • a hexyl group, a heptyl group, an octyl group, a nonyl group and a decyl group are preferred, and a hexyl group and an octyl group are more preferred.
  • mh represents an integer of 0 to 4, preferably an integer of 1 to 3, more preferably 2.
  • maleimide resin examples include the following compounds (h-1) to (h-4). However, (H) the maleimide resin is not limited to these specific examples. In the formula, nh represents an integer of 1-10.
  • maleimide resin examples include "BMI1500” manufactured by Designer Molecules, “SLK-1500-T80” manufactured by Shin-Etsu Chemical Co., Ltd. (compound of formula (h-1)); (h-2) compound); “BMI3000J” (compound of formula (h-3)); “BMI689” manufactured by Designer Molecules and “SLK-6895-T90” manufactured by Shin-Etsu Chemical Co., Ltd.
  • (H) maleimide resins also include maleimide resins (maleimide resins containing an indane ring skeleton) disclosed in Technical Bulletin No. 2020-500211 of Japan Institute of Invention and Innovation.
  • the weight average molecular weight (Mw) of the maleimide resin is preferably 150-5000, more preferably 300-2500.
  • the maleimide group equivalent of the maleimide resin is preferably 50 g/eq. ⁇ 2000 g/eq. , more preferably 100 g/eq. ⁇ 1000g/eq. , more preferably 150 g/eq. ⁇ 500 g/eq. is.
  • the maleimide group equivalent weight represents the weight of the (H) maleimide resin containing one equivalent maleimide group.
  • the amount of the (H) maleimide resin in the resin composition may be 0% by mass or greater than 0% by mass, preferably 0.0% by mass, relative to 100% by mass of non-volatile components in the resin composition. 01% by mass or more, more preferably 0.02% by mass or more, particularly preferably 0.03% by mass or more, preferably 5% by mass or less, more preferably 2% by mass or less, and particularly preferably 1% by mass or less. be.
  • the amount of the maleimide resin is within the above range, the dielectric loss tangent of the cured product of the resin composition can be particularly effectively reduced.
  • the amount of the (H) maleimide resin in the resin composition may be 0% by mass, may be greater than 0% by mass, and is preferably 0.01 with respect to 100% by mass of the resin component of the resin composition. % by mass or more, more preferably 0.05% by mass or more, particularly preferably 0.1% by mass or more, preferably 5% by mass or less, more preferably 2% by mass or less, and particularly preferably 1% by mass or less .
  • the amount of the maleimide resin is within the above range, the dielectric loss tangent of the cured product of the resin composition can be particularly effectively reduced.
  • the resin composition according to the present embodiment may further contain (I) an optional additive as an optional non-volatile component in combination with the components (A) to (H) described above.
  • Optional additives include, for example, thermosetting resins other than epoxy resins; organic fillers such as rubber particles; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; phthalocyanine blue, phthalocyanine Colorants such as green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; Thickeners such as bentone and montmorillonite; Antifoaming agents such as silicone antifoaming agents, acrylic antifoaming agents, fluorine antifoaming agents, and vinyl resin antifoaming agents;
  • melamine sulfate melamine sulfate
  • halogen flame retardants e.g. antimony trioxide
  • phosphate ester dispersants polyoxyalkylene dispersants, acetylene dispersants, silicone dispersants Dispersants such as agents, anionic dispersants, cationic dispersants; borate stabilizers, titanate stabilizers, aluminate stabilizers, zirconate stabilizers, isocyanate stabilizers, carboxylic acid stabilizers, carboxylic acid stabilizers stabilizers such as anhydride-based stabilizers.
  • Optional additives may be used singly or in combination of two or more.
  • the resin composition according to the present embodiment may contain (J) a solvent as an optional volatile component in combination with the non-volatile components such as components (A) to (I) described above.
  • a solvent an organic solvent is usually used.
  • organic solvents examples include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone; ester solvents; ether solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole; alcohol solvents such as methanol, ethanol, propanol, butanol, ethylene glycol; acetic acid Ether ester solvents such as 2-ethoxyethyl, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, ⁇ -butyrolactone, methyl methoxypropionate; methyl lactate, ethyl lactate, methyl 2-hydroxyisobutyrate, etc.
  • ester alcohol solvents 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, diethylene glycol monobutyl ether (butyl carbitol) and other ether alcohol solvents; N,N-dimethylformamide, N, Amide solvents such as N-dimethylacetamide and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethylsulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatics such as hexane, cyclopentane, cyclohexane, and methylcyclohexane Hydrocarbon-based solvents: aromatic hydrocarbon-based solvents such as benzene, toluene, xylene, ethylbenzene, trimethylbenzene, and the like can be mentioned. (J) The solvent may be used alone or in combination of two or more.
  • the amount of the solvent is not particularly limited, but is, for example, 60% by mass or less, 40% by mass or less, 30% by mass or less, or 20% by mass with respect to 100% by mass of all components of the resin composition. Thereafter, it may be 15% by mass or less, 10% by mass or less, or the like, and may be 0% by mass.
  • the resin composition according to this embodiment can be produced, for example, by mixing the components described above. Some or all of the components described above may be mixed at the same time, or may be mixed in order. During the course of mixing each component, the temperature may be set accordingly, and thus may be temporarily or permanently heated and/or cooled. Moreover, you may perform stirring or shaking in the process of mixing each component.
  • a cured product having a low dielectric loss tangent can be obtained from the resin composition according to the present embodiment.
  • a low dielectric loss tangent can be obtained when the dielectric loss tangent of a cured product of the resin composition is measured under the conditions described in [Test Example 1: Measurement of dielectric loss tangent] in Examples described later.
  • the dielectric loss tangent of the cured product is preferably 0.0040 or less, more preferably 0.0035 or less, still more preferably 0.0033 or less, and particularly preferably 0.0030 or less.
  • the lower limit is not particularly limited, and can be, for example, 0.0010 or more.
  • the resin composition according to this embodiment it is possible to obtain a cured product capable of suppressing the occurrence of cracks.
  • the yield is measured as an index of the frequency of occurrence of cracks in the cured product of the resin composition under the conditions described in [Test Example 2: Crack Evaluation Test] in Examples described later, the yield is preferably 40% or more, More preferably 60% or more, particularly preferably 80% or more.
  • a cured product having a high elongation at break can be obtained from the resin composition according to the present embodiment.
  • the elongation at break of the cured product is preferably 1.2% or more, more preferably 1.4% or more, and particularly preferably 1.6% or more.
  • the upper limit is not particularly limited, and may be, for example, 10% or less.
  • the resin composition according to the present embodiment can be used as a resin composition for insulation, and in particular can be suitably used as a resin composition for forming an insulation layer (resin composition for forming an insulation layer).
  • the resin composition according to the present embodiment can be used as a resin composition for forming an insulating layer of a printed wiring board, and a resin composition for forming an interlayer insulating layer (resin composition for interlayer insulation). can be suitably used as
  • the resin composition according to the present embodiment may be used as a resin composition for forming a rewiring layer (resin composition for forming a rewiring layer).
  • a rewiring formation layer represents an insulating layer for forming a rewiring layer.
  • the rewiring layer represents a conductor layer formed on a rewiring forming layer as an insulating layer.
  • the resin composition according to the present embodiment may be used as a resin composition for forming a rewiring layer.
  • a rewiring layer may be further formed on the sealing layer.
  • the resin composition according to the present embodiment includes, for example, a resin sheet, a sheet-like laminated material such as prepreg, a solder resist, an underfill material, a die bonding material, a semiconductor sealing material, a hole-filling resin, a part-embedding resin, etc. It can be used in a wide range of applications in which the composition is used.
  • the resin composition according to the present embodiment may be applied in the form of a varnish, it is industrially preferable to use it in the form of a sheet-like laminated material containing the resin composition.
  • the resin sheets and prepregs shown below are preferable.
  • the resin sheet includes a support and a resin composition layer provided on the support.
  • the resin composition layer is formed of the resin composition according to this embodiment. Therefore, the resin composition layer usually contains the resin composition, and preferably contains only the resin composition.
  • the thickness of the resin composition layer is preferably 50 ⁇ m or less, more It is preferably 40 ⁇ m or less.
  • the lower limit of the thickness of the resin composition layer is not particularly limited, but may be 5 ⁇ m or more, 10 ⁇ m or more, or the like.
  • the support examples include a film made of a plastic material, a metal foil, and a release paper, and a film made of a plastic material and a metal foil are preferable.
  • plastic material examples include polyethylene terephthalate (hereinafter sometimes abbreviated as "PET”) and polyethylene naphthalate (hereinafter sometimes abbreviated as “PEN”).
  • PET polyethylene terephthalate
  • PEN polyethylene naphthalate
  • PC polycarbonate
  • acrylic such as polymethyl methacrylate (PMMA)
  • PMMA polymethyl methacrylate
  • TAC triacetyl cellulose
  • PES polyether sulfide
  • polyether ketones polyimides, and the like.
  • polyethylene terephthalate and polyethylene naphthalate are preferable, and inexpensive polyethylene terephthalate is particularly preferable.
  • examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred.
  • a foil made of a single metal of copper may be used, and a foil made of an alloy of copper and other metals (for example, tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used. may be used.
  • the support may be subjected to matte treatment, corona treatment, or antistatic treatment on the surface to be bonded to the resin composition layer.
  • a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used.
  • the release agent used in the release layer of the release layer-attached support includes, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. .
  • a commercially available product may be used, for example, "SK-1” manufactured by Lintec Co., Ltd., “SK-1", “ AL-5”, “AL-7”, Toray's "Lumirror T60", Teijin's "Purex”, and Unitika's "Unipeel”.
  • the thickness of the support is not particularly limited, it is preferably in the range of 5 ⁇ m to 75 ⁇ m, more preferably in the range of 10 ⁇ m to 60 ⁇ m.
  • the thickness of the release layer-attached support as a whole is preferably within the above range.
  • the resin sheet may further contain any layer as necessary.
  • an optional layer include a protective film conforming to the support provided on the surface of the resin composition layer not bonded to the support (that is, the surface opposite to the support). be done.
  • the thickness of the protective film is not particularly limited, it is, for example, 1 ⁇ m to 40 ⁇ m. By laminating the protective film, it is possible to suppress adhesion of dust and scratches on the surface of the resin composition layer.
  • a liquid (varnish) resin composition is used as it is, or a liquid (varnish) resin composition is prepared by dissolving the resin composition in a solvent, and this is coated using a die coater or the like. It can be produced by coating on a support and further drying to form a resin composition layer.
  • Examples of the solvent include the same solvents as those described as components of the resin composition.
  • a solvent may be used individually by 1 type, and may be used in combination of 2 or more types.
  • Drying may be carried out by methods such as heating and blowing hot air.
  • drying conditions are not particularly limited, drying is performed so that the solvent content in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less.
  • the solvent content in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less.
  • the resin composition is dried at 50 ° C. to 150 ° C. for 3 minutes to 10 minutes. layer can be formed.
  • the resin sheet can be rolled up and stored.
  • the resin sheet has a protective film, it can be used by peeling off the protective film.
  • the prepreg is formed by impregnating a sheet-like fiber base material with the resin composition according to the present embodiment.
  • the thickness of the sheet-like fiber base material is preferably 50 ⁇ m or less, more preferably 40 ⁇ m or less, still more preferably 30 ⁇ m or less, and particularly preferably 20 ⁇ m or less.
  • the lower limit of the thickness of the sheet-like fiber base material is not particularly limited, and is usually 10 ⁇ m or more.
  • the prepreg can be manufactured by methods such as the hot melt method and the solvent method.
  • the thickness of the prepreg can be in the same range as the resin composition layer in the resin sheet described above.
  • the sheet-like laminated material can be suitably used for forming the insulating layer of the printed wiring board (for the insulating layer of the printed wiring board), and for forming the interlayer insulating layer of the printed wiring board (for the printed wiring board). for interlayer insulating layers).
  • a printed wiring board according to one embodiment of the present invention includes an insulating layer containing a cured product of the resin composition according to the present embodiment.
  • This printed wiring board can be manufactured, for example, using the resin sheet described above by a method including the following steps (I) and (II).
  • (II) A step of curing the resin composition layer to form an insulating layer.
  • the “inner layer substrate” used in step (I) is a member that serves as a printed wiring board substrate, and includes, for example, a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. etc.
  • the substrate may also have a conductor layer on one or both sides thereof, and the conductor layer may be patterned.
  • An inner layer substrate having conductor layers (circuits) formed on one side or both sides of the substrate is sometimes referred to as an "inner layer circuit board.”
  • an intermediate product on which an insulating layer and/or a conductor layer are further formed when manufacturing a printed wiring board is also included in the above-mentioned "inner layer board".
  • an inner layer board with built-in components may be used.
  • Lamination of the inner layer substrate and the resin sheet can be performed, for example, by heat-pressing the resin sheet to the inner layer substrate from the support side.
  • the member for thermocompression bonding the resin sheet to the inner layer substrate include heated metal plates (such as SUS end plates) and metal rolls (such as SUS rolls).
  • thermocompression member instead of pressing the thermocompression member directly onto the resin sheet, it is preferable to press through an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the uneven surface of the inner layer substrate.
  • Lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method.
  • the thermocompression temperature is preferably in the range of 60° C. to 160° C., more preferably 80° C. to 140° C.
  • the thermocompression pressure is preferably 0.098 MPa to 1.77 MPa, more preferably 0. .29 MPa to 1.47 MPa
  • the heat pressing time is preferably 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds.
  • Lamination is preferably carried out under reduced pressure conditions with a pressure of 26.7 hPa or less.
  • Lamination can be done with a commercially available vacuum laminator.
  • Commercially available vacuum laminators include, for example, a vacuum pressurized laminator manufactured by Meiki Seisakusho, a vacuum applicator manufactured by Nikko Materials, a batch vacuum pressurized laminator, and the like.
  • the laminated resin sheets may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side.
  • the pressing conditions for the smoothing treatment may be the same as the thermocompression bonding conditions for the lamination described above.
  • Smoothing treatment can be performed with a commercially available laminator. Lamination and smoothing may be performed continuously using the above-mentioned commercially available vacuum laminator.
  • the support may be removed between step (I) and step (II), or may be removed after step (II).
  • step (II) the resin composition layer is cured to form an insulating layer made of the cured resin composition.
  • Curing of the resin composition layer is usually performed by heat curing.
  • the specific curing conditions for the resin composition layer the conditions that are usually employed when forming the insulating layer of a printed wiring board may be used.
  • thermosetting conditions for the resin composition layer vary depending on the type of resin composition and the like. It is preferably 170°C to 210°C. Curing time may preferably be from 5 minutes to 120 minutes, more preferably from 10 minutes to 100 minutes, even more preferably from 15 minutes to 100 minutes.
  • the resin composition layer may be preheated at a temperature lower than the curing temperature before thermally curing the resin composition layer.
  • the resin composition layer is cured at a temperature of 50° C. to 150° C., preferably 60° C. to 140° C., more preferably 70° C. to 130° C. for 5 minutes or more, It may be preheated for preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, even more preferably 15 minutes to 100 minutes.
  • steps (III) to (V) may be carried out according to various methods known to those skilled in the art that are used in the manufacture of printed wiring boards.
  • the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or step ( It may be carried out between IV) and step (V). If necessary, the steps (I) to (V) of forming the insulating layer and the conductor layer may be repeated to form a multilayer wiring board.
  • a printed wiring board can be manufactured using the prepreg described above.
  • the manufacturing method can be basically the same as in the case of using a resin sheet.
  • the step (III) is a step of drilling holes in the insulating layer, whereby holes such as via holes and through holes can be formed in the insulating layer.
  • Step (III) may be performed using, for example, a drill, laser, plasma, or the like, depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined according to the design of the printed wiring board.
  • Step (IV) is a step of roughening the insulating layer. Smear is usually also removed in this step (IV).
  • the procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are commonly used in forming insulating layers of printed wiring boards can be employed.
  • the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralizing treatment with a neutralizing liquid in this order.
  • Examples of the swelling liquid used for the roughening treatment include alkaline solutions and surfactant solutions, preferably alkaline solutions.
  • As the alkaline solution a sodium hydroxide solution and a potassium hydroxide solution are more preferred.
  • Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU” manufactured by Atotech Japan.
  • the swelling treatment with a swelling liquid can be performed, for example, by immersing the insulating layer in a swelling liquid at 30° C. to 90° C. for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40° C. to 80° C. for 5 minutes to 15 minutes.
  • Examples of the oxidizing agent used for the roughening treatment include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide.
  • the roughening treatment with an oxidizing agent such as an alkaline permanganate solution is preferably carried out by immersing the insulating layer in an oxidizing agent solution heated to 60° C. to 100° C. for 10 to 30 minutes.
  • the permanganate concentration in the alkaline permanganate solution is preferably 5% by mass to 10% by mass.
  • Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Security P" manufactured by Atotech Japan.
  • the neutralizing solution used for roughening treatment is preferably an acidic aqueous solution, and commercially available products include, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan.
  • the treatment with the neutralizing solution can be carried out by immersing the treated surface roughened with the oxidizing agent in the neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method of immersing an object roughened with an oxidizing agent in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferable.
  • the arithmetic mean roughness (Ra) of the insulating layer surface after roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less.
  • the lower limit is not particularly limited, and can be, for example, 1 nm or more, 2 nm or more.
  • the root mean square roughness (Rq) of the surface of the insulating layer after roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less.
  • the lower limit is not particularly limited, and can be, for example, 1 nm or more, 2 nm or more.
  • the arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.
  • the step (V) is a step of forming a conductor layer, and forms the conductor layer on the insulating layer.
  • the conductor material used for the conductor layer is not particularly limited.
  • the conductor layer contains one or more selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. Contains metal.
  • the conductor layer may be a single metal layer or an alloy layer, and the alloy layer may be, for example, an alloy of two or more metals selected from the above group (for example, a nickel-chromium alloy, a copper- nickel alloys and copper-titanium alloys).
  • single metal layers of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, nickel-chromium alloys, copper- Nickel alloys and copper/titanium alloy alloy layers are preferred, and single metal layers of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or nickel/chromium alloy alloy layers are more preferred, and copper single metal layers are preferred.
  • a metal layer is more preferred.
  • the conductor layer may have a single layer structure, or may have a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated.
  • the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of nickel-chromium alloy.
  • the thickness of the conductor layer is generally 3 ⁇ m to 35 ⁇ m, preferably 5 ⁇ m to 30 ⁇ m, depending on the desired printed wiring board design.
  • the conductor layer may be formed by plating.
  • a conductive layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method.
  • a semi-additive method is preferable from the viewpoint of manufacturing simplicity.
  • An example of forming a conductor layer by a semi-additive method is shown below.
  • a plating seed layer is formed on the surface of the insulating layer by electroless plating.
  • a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to a desired wiring pattern.
  • the mask pattern is removed. After that, the unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern can be formed.
  • the conductor layer may be formed using metal foil.
  • step (V) is preferably performed between step (I) and step (II).
  • step (I) the support is removed and a metal foil is laminated on the exposed surface of the resin composition layer.
  • Lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for step (I).
  • step (II) is performed to form an insulating layer.
  • a conductor layer having a desired wiring pattern can be formed by conventional known techniques such as the subtractive method and the modified semi-additive method.
  • a metal foil can be manufactured by a known method such as an electrolysis method or a rolling method.
  • Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Co., Ltd., 3EC-III foil and TP-III foil manufactured by Mitsui Kinzoku Mining Co., Ltd., and the like.
  • a semiconductor device includes the printed wiring board described above.
  • a semiconductor device can be manufactured using a printed wiring board.
  • semiconductor devices examples include various semiconductor devices used in electrical products (such as computers, mobile phones, digital cameras, televisions, etc.) and vehicles (such as motorcycles, automobiles, trains, ships, aircraft, etc.).
  • Example 1 10 parts of a phenol-based curing agent having a biphenyl aralkyl structure (“GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g / eq.), and a biphenyl type epoxy resin (“NC-3000” manufactured by Nippon Kayaku Co., Ltd.) , an epoxy equivalent of about 275 g/eq.) was dissolved in 40 parts of MEK by heating with stirring to obtain a dissolved composition. This was cooled to room temperature, and 73 parts of an active ester compound ("HPC-8000-65T" manufactured by DIC, a toluene solution having an active ester group equivalent of about 223 g/eq.
  • GPH-65 phenol-65
  • NC-3000 manufactured by Nippon Kayaku Co., Ltd.
  • Example 2 The amount of spherical silica ("SO-C2" manufactured by Admatechs) was reduced to 200 parts by mass. Further, 49 parts by mass of hollow aluminosilicate particles ("MGH-005" manufactured by Taiheiyo Cement Co., Ltd., average particle diameter 1.6 ⁇ m, porosity 80% by volume) were added to the resin composition. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • SO-C2 spherical silica
  • MGH-005" manufactured by Taiheiyo Cement Co., Ltd., average particle diameter 1.6 ⁇ m, porosity 80% by volume
  • Example 3 The amount of spherical silica ("SO-C2" manufactured by Admatechs) was reduced to 200 parts by mass. Further, 11.2 parts by mass of hollow silica particles (average particle size: 2.6 ⁇ m, porosity: 25% by volume) were added to the resin composition. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 4 instead of 10 parts of a phenol compound having a biphenyl aralkyl structure ("GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g / eq.), a phenol compound having a biphenyl aralkyl structure ("GPH” manufactured by Nippon Kayaku Co., Ltd.) A resin composition (resin varnish) was prepared in the same manner as in Example 1, except for using 10 parts of "A-103" with a phenol equivalent of about 231 g/eq.
  • Example 5 The amount of a phenol compound having a biphenylaralkyl structure ("GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g/eq.) was reduced to 2 parts by mass. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 240 parts by mass. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Resin A composition (resin varnish) was prepared.
  • Example 7 Instead of 30 parts of biphenyl type epoxy resin ("NC-3000” manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 275 g / eq.) naphthalene type epoxy resin ("HP-4032-SS” manufactured by DIC Corporation, epoxy equivalent of about 145 g / eq.) was used to prepare a resin composition (resin varnish) in the same manner as in Example 1.
  • Example 8 Instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. toluene solution) was used. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 9 10 parts of a naphthalene-type phenol curing agent ("SN-485" phenol loading equivalent of about 215 g/eq. manufactured by Nippon Steel Chemical & Material) was added to the resin composition. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 288 parts. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • SN-485" phenol loading equivalent of about 215 g/eq. manufactured by Nippon Steel Chemical & Material was added to the resin composition. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 288 parts.
  • a resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 10 20 parts of a triazine skeleton-containing phenolic curing agent (“LA-3018-50P” manufactured by DIC, active group equivalent of about 151 g/eq., 2-methoxypropanol solution with a non-volatile content of 50%) was added to the resin composition. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 288 parts. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • LA-3018-50P manufactured by DIC, active group equivalent of about 151 g/eq., 2-methoxypropanol solution with a non-volatile content of 50%
  • Example 11 The amount of a phenolic compound having a biphenylaralkyl structure (“GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g/eq.) was increased to 25 parts. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 290 parts. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 12 Phenoxy resin ("YX7553BH30” manufactured by Mitsubishi Chemical Corporation, 1:1 solution of MEK and cyclohexanone with a nonvolatile content of 30% by mass) instead of 0.2 parts, cyclohexane ring-containing maleimide resin (manufactured by Shin-Etsu Chemical Co., Ltd. "SLK-6895- A resin composition (resin varnish) was prepared in the same manner as in Example 1, except that 0.2 part of T90", a toluene solution with a non-volatile content of 90% by mass) was used.
  • Example 13 Instead of 10 parts of a phenol compound having a biphenyl aralkyl structure ("GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g / eq.), a phenol compound having a biphenyl aralkyl structure ("GPH” manufactured by Nippon Kayaku Co., Ltd.) -103", phenol equivalent of about 231 g/eq.) was used. In addition, instead of 73 parts of the active ester compound (“HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq.
  • HPC-8000-65T manufactured by DIC
  • HPC-8150-62T manufactured by DIC
  • Example 14 The amount of a phenolic compound having a biphenylaralkyl structure (“GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g/eq.) was increased to 25 parts. In addition, instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. 73 parts of a 62% toluene solution) were used. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 285 parts by mass. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 15 Instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. toluene solution) was used. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 282 parts by mass. Furthermore, 20 parts of a triazine skeleton-containing phenolic curing agent (“LA-3018-50P” manufactured by DIC, active group equivalent of about 151 g/eq., 2-methoxypropanol solution with a nonvolatile content of 50%) is added to the resin composition. bottom. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 16 Instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. toluene solution) was used. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass.
  • a cyclohexane ring-containing maleimide resin manufactured by Shin-Etsu Chemical Co., Ltd. "SLK- 6895-T90", a toluene solution with a nonvolatile content of 90% by mass
  • a resin composition was prepared in the same manner as in Example 1 except for the above matters.
  • Example 17 The amount of a phenolic compound having a biphenylaralkyl structure (“GPH-65” manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g/eq.) was increased to 25 parts. In addition, instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. 73 parts of a 62% toluene solution) were used. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 285 parts by mass.
  • GPH-65 phenolic compound having a biphenylaralkyl structure manufactured by Nippon Kayaku Co., Ltd., phenol equivalent of about 198 g/eq.
  • cyclohexane ring-containing maleimide resin manufactured by Shin-Etsu Chemical Co., Ltd. "SLK- 6895-T90", a toluene solution with a nonvolatile content of 90% by mass
  • a resin composition was prepared in the same manner as in Example 1 except for the above matters.
  • Example 18 Instead of 30 parts of biphenyl type epoxy resin ("NC-3000” manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 275 g / eq.) naphthalene type epoxy resin ("HP-4032-SS” manufactured by DIC Corporation, epoxy equivalent of about 145 g / eq.) 30 parts were used. In addition, instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. 73 parts of a 62% toluene solution) were used. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 20 Instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. toluene solution) was used. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass.
  • Example 21 Instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. toluene solution) was used. Also, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 285 parts by mass. Furthermore, 20 parts of a triazine skeleton-containing phenolic curing agent (“LA-3018-50P” manufactured by DIC, active group equivalent of about 151 g/eq., 2-methoxypropanol solution with a nonvolatile content of 50%) is added to the resin composition. bottom.
  • HPC-8150-62T manufactured by DIC
  • SO-C2 spherical silica
  • LA-3018-50P manufactured by DIC, active group equivalent of about 151 g/eq., 2-methoxypropanol solution with a nonvol
  • Example 22 Instead of 30 parts of biphenyl type epoxy resin ("NC-3000” manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 275 g / eq.) naphthalene type epoxy resin ("HP-4032-SS” manufactured by DIC Corporation, epoxy equivalent of about 145 g / eq.) 30 parts were used. In addition, instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), a different active ester compound (“HPC-8150-62T” manufactured by DIC) with an active ester group equivalent of about 229 g/eq. 73 parts of a 62% toluene solution) were used.
  • the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 258 parts by mass.
  • the amount of phenoxy resin (“YX7553BH30” manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone having a nonvolatile content of 30% by mass) was increased to 1 part by mass.
  • 1 part of a maleimide resin (“SLK-1500-T80” manufactured by Shin-Etsu Chemical Co., Ltd., a toluene solution containing 80% by mass of non-volatile components) was added to the resin composition.
  • a resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 23 Instead of 30 parts of biphenyl type epoxy resin ("NC-3000” manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 275 g / eq.) naphthalene type epoxy resin ("HP-4032-SS” manufactured by DIC Corporation, epoxy equivalent of about 145 g / eq.) 30 parts were used. Further, instead of 73 parts of the active ester compound ("HPC-8000-65T” manufactured by DIC), 52 parts of the active ester compound (“HPC-8000-65T” manufactured by DIC) and an active ester compound (“HPC manufactured by DIC”) -8150-62T" with an active ester group equivalent of about 229 g/eq. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass. A resin composition (resin varnish) was prepared in the same manner as in Example 1 except for the above matters.
  • Example 24 Instead of 73 parts of the active ester compound (manufactured by DIC “HPC-8000-65T”), 35 parts of the active ester compound (manufactured by DIC “HPC-8000-65T”) and the active ester compound (manufactured by DIC "HPC-8150 -62T” with an active ester group equivalent of about 229 g/eq. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was increased to 285 parts by mass.
  • SO-C2 spherical silica
  • Example 25 Instead of 73 parts of the active ester compound (manufactured by DIC “HPC-8000-65T”), 18 parts of the active ester compound (manufactured by DIC “HPC-8000-65T”) and the active ester compound (manufactured by DIC "HPC-8150 -62T” with an active ester group equivalent of about 229 g/eq. Furthermore, the amount of spherical silica (“SO-C2" manufactured by Admatechs) was reduced to 255 parts by mass.
  • SO-C2 spherical silica
  • cyclohexane ring-containing maleimide resin manufactured by Shin-Etsu Chemical Co., Ltd. "SLK- 6895-T90", a toluene solution with a nonvolatile content of 90% by mass
  • a resin composition was prepared in the same manner as in Example 1 except for the above matters.
  • a polyethylene terephthalate film (“Lumirror R80” manufactured by Toray Industries, Inc.; thickness 38 ⁇ m, softening point 130° C.) whose surface was subjected to release treatment with an alkyd resin release agent (“AL-5” manufactured by Lintec).
  • the resin composition was uniformly coated on the support so that the thickness of the resin composition layer after drying was 40 ⁇ m, and dried at 90° C. for 3 minutes.
  • a polyethylene terephthalate film similar to the support is attached as a protective film to the exposed surface of the resin composition layer (the surface not bonded to the support) to obtain a layer structure of support/resin composition layer/protective film.
  • the value of dielectric loss tangent was measured by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C using "HP8362B" manufactured by Agilent Technologies. Three test pieces were measured, and the average value was calculated.
  • Such lamination is carried out using a vacuum pressure laminator (“MVLP-500” manufactured by Meiki Seisakusho Co., Ltd.), vacuuming at a temperature of 120° C. for 30 seconds, and then supporting under conditions of a temperature of 120° C. and a pressure of 7.0 kg/cm 2 . It was carried out by pressing for 30 seconds from the body via a heat-resistant rubber. Next, under atmospheric pressure, pressing was performed for 60 seconds under the conditions of a temperature of 120° C. and a pressure of 5.5 kg/cm 2 using SUS end plates.
  • MVLP-500 manufactured by Meiki Seisakusho Co., Ltd.
  • the support was peeled off from the laminated resin sheet. Using a hot air circulating furnace, the resin composition layer was thermally cured under thermal curing conditions of 170° C. for 30 minutes to form an insulating layer. Thus, a sample substrate having a layer structure of inner layer substrate/insulating layer was obtained. Next, the sample substrate was left to cool to room temperature (25° C.).
  • the sample substrate was immersed in an oxidizing agent ("Concentrate Compact CP” manufactured by Atotech Japan) at 80°C for 20 minutes. Further, the sample substrate was immersed in a neutralizing solution (“Reduction Solution Securigant P” manufactured by Atotech Japan) at 40° C. for 5 minutes. After that, the sample substrate was dried at 80° C. for 30 minutes.
  • an oxidizing agent (“Concentrate Compact CP” manufactured by Atotech Japan) at 80°C for 20 minutes.
  • a neutralizing solution (“Reduction Solution Securigant P” manufactured by Atotech Japan) at 40° C. for 5 minutes. After that, the sample substrate was dried at 80° C. for 30 minutes.
  • ⁇ Crack evaluation method> Of the insulating layer surface of the sample substrate after desmearing, the L/S pattern of the inner layer substrate was observed. In 100 portions on the pattern of the inner layer substrate, it was confirmed whether cracks occurred on the surface along the pattern shape, and the number of portions on the pattern where no cracks occurred was counted. The percentage of crack-free parts out of 100 parts was calculated as the "yield". A higher yield is more preferable. Therefore, the calculated yield was scored according to the following criteria. 1 point: 0% or more and less than 20%. 2 points: 20% or more and less than 40%. 3 points: 40% or more and less than 60%. 4 points: 60% or more and less than 80%. 5 points: 80% or more. Three points or more were determined as crack evaluation " ⁇ ". In addition, 2 points or less was determined to be crack evaluation "x".
  • Test Example 3 Measurement of elongation at break
  • the cured product A for evaluation obtained in Test Example 1 was subjected to a tensile test using a Tensilon universal testing machine (“RTC-1250A” manufactured by Orientec Co., Ltd.) in accordance with Japanese Industrial Standards JIS K7127, and the elongation at break ( %) was measured.
  • RTC-1250A Tensilon universal testing machine
  • Active ester group/epoxy group Number of active ester groups of (C) active ester compound when the number of epoxy groups of (B) epoxy resin is 1.
  • Example 1 to 25 in which the components (A) to (D) were combined, all showed good results in dielectric loss tangent, cracking test and elongation at break. Considering that the dielectric loss tangent can be lowered in Example 1 compared to Example 11, which has a large amount of (A) biphenylaralkyl-type phenolic resin, the amount of (A) biphenylaralkyl-type phenolic resin reduces the dielectric loss tangent It can be seen that there are preferred ranges above.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Microelectronics & Electronic Packaging (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Epoxy Resins (AREA)
PCT/JP2022/037690 2021-10-14 2022-10-07 樹脂組成物 Ceased WO2023063266A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2023554505A JPWO2023063266A1 (cg-RX-API-DMAC7.html) 2021-10-14 2022-10-07
CN202280068015.4A CN118076697A (zh) 2021-10-14 2022-10-07 树脂组合物
KR1020247011930A KR20240087832A (ko) 2021-10-14 2022-10-07 수지 조성물

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021169102 2021-10-14
JP2021-169102 2021-10-14

Publications (1)

Publication Number Publication Date
WO2023063266A1 true WO2023063266A1 (ja) 2023-04-20

Family

ID=85987716

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/037690 Ceased WO2023063266A1 (ja) 2021-10-14 2022-10-07 樹脂組成物

Country Status (5)

Country Link
JP (1) JPWO2023063266A1 (cg-RX-API-DMAC7.html)
KR (1) KR20240087832A (cg-RX-API-DMAC7.html)
CN (1) CN118076697A (cg-RX-API-DMAC7.html)
TW (1) TW202336074A (cg-RX-API-DMAC7.html)
WO (1) WO2023063266A1 (cg-RX-API-DMAC7.html)

Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2018172519A (ja) * 2017-03-31 2018-11-08 住友ベークライト株式会社 熱硬化性樹脂組成物、キャリア付樹脂膜、プリプレグ、プリント配線基板および半導体装置
JP2020083898A (ja) * 2018-11-14 2020-06-04 味の素株式会社 樹脂組成物、樹脂シート、プリント配線板及び半導体装置
JP2020152825A (ja) * 2019-03-20 2020-09-24 日立化成株式会社 封止用樹脂組成物、電子部品装置及び電子部品装置の製造方法
JP2021014545A (ja) * 2019-07-12 2021-02-12 味の素株式会社 樹脂組成物
JP2021116331A (ja) * 2020-01-23 2021-08-10 昭和電工マテリアルズ株式会社 封止用樹脂組成物、電子部品装置、及び電子部品装置の製造方法
JP2021134300A (ja) * 2020-02-27 2021-09-13 味の素株式会社 樹脂組成物
JP2021161205A (ja) * 2020-03-31 2021-10-11 味の素株式会社 樹脂組成物、樹脂組成物の硬化物、樹脂シート、プリント配線板、半導体チップパッケージ及び半導体装置

Family Cites Families (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2020023714A (ja) 2019-10-24 2020-02-13 積水化学工業株式会社 樹脂材料及び多層プリント配線板

Patent Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2018172519A (ja) * 2017-03-31 2018-11-08 住友ベークライト株式会社 熱硬化性樹脂組成物、キャリア付樹脂膜、プリプレグ、プリント配線基板および半導体装置
JP2020083898A (ja) * 2018-11-14 2020-06-04 味の素株式会社 樹脂組成物、樹脂シート、プリント配線板及び半導体装置
JP2020152825A (ja) * 2019-03-20 2020-09-24 日立化成株式会社 封止用樹脂組成物、電子部品装置及び電子部品装置の製造方法
JP2021014545A (ja) * 2019-07-12 2021-02-12 味の素株式会社 樹脂組成物
JP2021116331A (ja) * 2020-01-23 2021-08-10 昭和電工マテリアルズ株式会社 封止用樹脂組成物、電子部品装置、及び電子部品装置の製造方法
JP2021134300A (ja) * 2020-02-27 2021-09-13 味の素株式会社 樹脂組成物
JP2021161205A (ja) * 2020-03-31 2021-10-11 味の素株式会社 樹脂組成物、樹脂組成物の硬化物、樹脂シート、プリント配線板、半導体チップパッケージ及び半導体装置

Also Published As

Publication number Publication date
KR20240087832A (ko) 2024-06-19
TW202336074A (zh) 2023-09-16
CN118076697A (zh) 2024-05-24
JPWO2023063266A1 (cg-RX-API-DMAC7.html) 2023-04-20

Similar Documents

Publication Publication Date Title
JP2022108928A (ja) 樹脂組成物
TW202235531A (zh) 樹脂組成物
JP2023165263A (ja) 樹脂組成物
WO2023149521A1 (ja) 樹脂組成物、硬化物、シート状積層材料、樹脂シート、プリント配線板、及び半導体装置
KR20230063875A (ko) 수지 조성물
JP2022108927A (ja) 樹脂組成物
JP2022150798A (ja) 樹脂組成物
TW202430594A (zh) 樹脂組成物
JP7311064B2 (ja) 樹脂組成物
JP7689142B2 (ja) 樹脂組成物
KR20230063871A (ko) 수지 조성물
JP7700456B2 (ja) 樹脂組成物
JP2023069752A (ja) 樹脂組成物
JP2022109004A (ja) 樹脂組成物
JP7754074B2 (ja) 樹脂組成物層
JP7472839B2 (ja) 樹脂組成物
WO2023203906A1 (ja) 樹脂組成物
TW202328322A (zh) 樹脂組成物
JP2022151212A (ja) プリント配線板の製造方法
JP2023124504A (ja) 樹脂組成物
JP2023003393A (ja) 樹脂組成物
JP7826647B2 (ja) 樹脂組成物
KR20240087832A (ko) 수지 조성물
KR20240028939A (ko) 수지 조성물
JP2023100523A (ja) 樹脂組成物

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22880961

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2023554505

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 202280068015.4

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 22880961

Country of ref document: EP

Kind code of ref document: A1