WO2023058355A1 - ヘテロエピタキシャル膜の作製方法 - Google Patents

ヘテロエピタキシャル膜の作製方法 Download PDF

Info

Publication number
WO2023058355A1
WO2023058355A1 PCT/JP2022/032016 JP2022032016W WO2023058355A1 WO 2023058355 A1 WO2023058355 A1 WO 2023058355A1 JP 2022032016 W JP2022032016 W JP 2022032016W WO 2023058355 A1 WO2023058355 A1 WO 2023058355A1
Authority
WO
WIPO (PCT)
Prior art keywords
single crystal
film
sic
heteroepitaxial
sic single
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/032016
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
剛 大槻
和徳 萩本
順也 石崎
達夫 阿部
温 鈴木
寿樹 松原
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shin-Etsu Handotai Co Ltd
Original Assignee
Shin-Etsu Handotai Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shin-Etsu Handotai Co Ltd filed Critical Shin-Etsu Handotai Co Ltd
Priority to CN202280067121.0A priority Critical patent/CN118176329A/zh
Priority to US18/695,073 priority patent/US20250163609A1/en
Priority to EP22878226.4A priority patent/EP4414483B1/en
Priority to JP2023552739A priority patent/JP7708198B2/ja
Priority to KR1020247010927A priority patent/KR102957204B1/ko
Publication of WO2023058355A1 publication Critical patent/WO2023058355A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B25/00—Single-crystal growth by chemical reaction of reactive gases, e.g. chemical vapour-deposition growth
    • C30B25/02—Epitaxial-layer growth
    • C30B25/16—Controlling or regulating
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/02—Pretreatment of the material to be coated
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/32—Carbides
    • C23C16/325—Silicon carbide
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/42—Silicides
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/56—After-treatment
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B25/00—Single-crystal growth by chemical reaction of reactive gases, e.g. chemical vapour-deposition growth
    • C30B25/02—Epitaxial-layer growth
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B25/00—Single-crystal growth by chemical reaction of reactive gases, e.g. chemical vapour-deposition growth
    • C30B25/02—Epitaxial-layer growth
    • C30B25/16—Controlling or regulating
    • C30B25/165—Controlling or regulating the flow of the reactive gases
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B25/00—Single-crystal growth by chemical reaction of reactive gases, e.g. chemical vapour-deposition growth
    • C30B25/02—Epitaxial-layer growth
    • C30B25/18—Epitaxial-layer growth characterised by the substrate
    • C30B25/186—Epitaxial-layer growth characterised by the substrate being specially pre-treated by, e.g. chemical or physical means
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B29/00—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape
    • C30B29/02—Elements
    • C30B29/06—Silicon
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B29/00—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape
    • C30B29/10—Inorganic compounds or compositions
    • C30B29/36—Carbides
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B29/00—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape
    • C30B29/10—Inorganic compounds or compositions
    • C30B29/40—AIIIBV compounds wherein A is B, Al, Ga, In or Tl and B is N, P, As, Sb or Bi
    • C30B29/403—AIII-nitrides
    • C30B29/406—Gallium nitride
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B29/00—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape
    • C30B29/60—Single crystals or homogeneous polycrystalline material with defined structure characterised by the material or by their shape characterised by shape
    • C30B29/68—Crystals with laminate structure, e.g. "superlattices"
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B33/00—After-treatment of single crystals or homogeneous polycrystalline material with defined structure
    • C—CHEMISTRY; METALLURGY
    • C30—CRYSTAL GROWTH
    • C30B—SINGLE-CRYSTAL GROWTH; UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL; PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; APPARATUS THEREFOR
    • C30B33/00—After-treatment of single crystals or homogeneous polycrystalline material with defined structure
    • C30B33/06—Joining of crystals
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/24—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials using chemical vapour deposition [CVD]
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/29—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by the substrates
    • H10P14/2901—Materials
    • H10P14/2902—Materials being Group IVA materials
    • H10P14/2905—Silicon, silicon germanium or germanium
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/29—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by the substrates
    • H10P14/2926—Crystal orientations
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/32—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by intermediate layers between substrates and deposited layers
    • H10P14/3202—Materials thereof
    • H10P14/3204—Materials thereof being Group IVA semiconducting materials
    • H10P14/3208—Silicon carbide
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/34—Deposited materials, e.g. layers
    • H10P14/3402—Deposited materials, e.g. layers characterised by the chemical composition
    • H10P14/3404—Deposited materials, e.g. layers characterised by the chemical composition being Group IVA materials
    • H10P14/3408—Silicon carbide
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/36—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by treatments done before the formation of the materials
    • H10P14/3602—In-situ cleaning
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/32—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by intermediate layers between substrates and deposited layers
    • H10P14/3242—Structure
    • H10P14/3244—Layer structure
    • H10P14/3248—Layer structure consisting of two layers
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/34—Deposited materials, e.g. layers
    • H10P14/3402—Deposited materials, e.g. layers characterised by the chemical composition
    • H10P14/3414—Deposited materials, e.g. layers characterised by the chemical composition being group IIIA-VIA materials
    • H10P14/3416—Nitrides
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/38—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by treatments done after the formation of the materials

Definitions

  • the present invention relates to a method for producing a heteroepitaxial film.
  • CMOS Complementary Metal Oxide Silicon
  • IGBT Insulated Gate Bipolar Transistor
  • chip-on-wafer integration in which cut-out elements are attached to a wafer on which metal wiring has been provided in advance, has been adopted. Also in this case, the cut out element is thinned and most of the silicon substrate is removed.
  • SiC has a wide bandgap of 2.2 to 3.3 eV compared to Si of 1.1 eV, so it has high dielectric breakdown strength. It is a material expected as a semiconductor material for various semiconductor devices.
  • Patent Documents 1, 2 and 3 propose a technique in which ions such as hydrogen are implanted into SiC or silicon and the substrate is separated from the implanted layer. With these methods, after peeling, the thin film side can be reused as a device, and the thick film side can be reused as a substrate (although surface polishing is required), which is a highly advantageous method.
  • these methods delaminate by creating a fragile layer by implanting ions such as hydrogen. It is extremely difficult to form a brittle layer at the beginning of the process. There are hurdles to commercialization.
  • JP 2010-251724 A Japanese Unexamined Patent Application Publication No. 2011-223011 Japanese Patent Publication No. 2010-502023
  • the present invention has been made to solve the above problems, and is to efficiently obtain a thin heteroepitaxial film with less damage to the device and less material loss.
  • the present invention includes a step of separating the 3C-SiC single crystal film from the single crystal silicon substrate after heteroepitaxially growing the 3C-SiC single crystal film on the single crystal silicon substrate.
  • a method for producing a heteroepitaxial film Using a reduced pressure CVD apparatus, a first step of removing a native oxide film on the surface of the single crystal silicon substrate by hydrogen baking; A second step of forming nuclei of SiC on the single crystal silicon substrate under conditions of a pressure of 1333 Pa or less and a temperature of 300° C. or more and 950° C. or less while supplying a source gas containing carbon and silicon into the low pressure CVD apparatus.
  • a SiC single crystal is grown under the conditions of a pressure of 1333 Pa or less and a temperature of 800° C. or more and less than 1200° C. to form a 3C—SiC single crystal film, and vacancies are formed immediately below the 3C—SiC single crystal film.
  • a method for fabricating a heteroepitaxial film comprising:
  • SiC nuclei can be formed in the second step.
  • a heteroepitaxial film having a high-quality 3C-SiC single crystal film can be obtained. Wafers can be manufactured efficiently.
  • the pressure to 1333 Pa (10 Torr) or less, it is possible to prevent the occurrence of secondary or higher-order reactions, such as reaction of the reactive species with the raw material gas in the vapor phase, thereby enabling heteroepitaxial growth. can be made certain.
  • vacancies are formed in the silicon layer (single crystal silicon substrate) directly below the 3C-SiC single crystal film (hereinafter also referred to as the 3C-SiC/silicon interface).
  • the presence of these vacancies not only alleviates the lattice mismatch between 3C-SiC and silicon, but also alleviates the stress in the entire epitaxial layer, so even a thick 3C-SiC single crystal film It also becomes possible to more reliably form a 3C-SiC single crystal film free of crystal defects.
  • 3C-SiC A heteroepitaxial wafer having a single crystal film can be efficiently obtained. Furthermore, by separating and exfoliating at the vacancies at the 3C-SiC/silicon interface in the fourth step, it is possible to efficiently obtain the desired heteroepitaxial film containing the 3C-SiC single crystal film. Moreover, since the separation is at the 3C-SiC/silicon interface, the single crystal silicon substrate can be separated with little loss. That is, a thicker single crystal silicon substrate can be obtained after separation, which is effective in terms of reuse. Also, even if the device is formed on the 3C—SiC single crystal film and then peeled off, the damage to the device is small.
  • monomethylsilane or trimethylsilane can be used as the source gas.
  • the first step can be performed under the condition that the temperature is 1000°C or higher and 1200°C or lower.
  • the natural oxide film on the surface of the single crystal silicon substrate can be removed more efficiently, and the 3C-SiC single crystal film can be formed more reliably. Also, the occurrence of slip dislocations can be prevented.
  • the third step can be performed under the condition that the pressure is 133 Pa or less.
  • vacancies can be more reliably formed at the 3C-SiC/silicon interface while growing the 3C-SiC single crystal film.
  • the 3C—SiC single crystal film (heteroepitaxial film) can be separated more reliably in the fourth step.
  • the third step can be performed with one or more of pressure and temperature higher than the conditions of the second step.
  • the growth rate of the 3C—SiC single crystal film can be increased in the third step by doing so. , it is possible to efficiently form a thick 3C-SiC single crystal film.
  • the third step can be performed at a temperature of 1000°C or more and less than 1200°C.
  • the single-crystal silicon substrate is grown. It is not subject to restrictions that limit the plane orientation of It is possible to more reliably grow a 3C-SiC single crystal film by ion implantation without forming a fragile layer such as hydrogen. Furthermore, a 3C—SiC single crystal film can be more easily formed on a large diameter single crystal silicon substrate such as 300 mm in diameter.
  • one or more of pressure and temperature can be increased during the third step.
  • the pressure in the initial stage of the third step, for example, can be set to 133 Pa (1 Torr) or less, and then the pressure can be increased to increase the deposition rate.
  • the film formation speed can be increased by increasing the temperature from the middle.
  • the second step and the third step are performed under conditions in which the temperature is gradually increased from the range of 300° C. or higher and 950° C. or lower to the range of 1000° C. or higher and lower than 1200° C.
  • the formation of the SiC nuclei and the formation of the 3C-SiC single crystal film following the formation of the SiC nuclei can be carried out continuously.
  • the heteroepitaxial growth is rate-determining the transport of the supply gas, the limitation of the plane orientation of the single-crystal silicon substrate can be avoided, and the necessity of containing hydrogen can be eliminated. can. In addition, it becomes easier to form a 3C-SiC single crystal film on a large diameter single crystal silicon substrate.
  • the temperature increase can be performed at a temperature increase rate of 0.5°C/sec or more and 2°C/sec or less.
  • GaN may be further grown on the surface of the formed 3C—SiC single crystal film to form a GaN layer, or the third step.
  • a Si layer can be formed by further growing Si on the surface of the formed 3C-SiC single crystal film.
  • the 3C-SiC single crystal film grown as described above has a flat surface, a GaN layer and a Si layer can be heteroepitaxially grown on the surface of the 3C-SiC single crystal film.
  • the fourth step can be performed after forming a protective film on the formed 3C-SiC single crystal film.
  • a device may be formed on the formed 3C—SiC single crystal film, a protective film may be formed, and then the fourth step may be performed.
  • a protective film is formed after cutting out the device along the scribe line of the device, and then the fourth step is performed. It can be carried out.
  • the 3C-SiC single crystal film can be peeled off as it is, or it can be peeled off after the device is formed.
  • heteroepitaxial film manufacturing method of the present invention 3C such that vacancies are generated in the silicon substrate (3C-SiC/silicon interface) while maintaining good 3C-SiC single crystallinity on the single crystal silicon substrate.
  • a thin heteroepitaxial film can be efficiently obtained by efficiently performing heteroepitaxial growth of a -SiC single crystal film and peeling off the 3C-SiC single crystal film from the silicon substrate using the vacancies.
  • it is extremely effective in terms of damage to devices and loss of materials.
  • SiC as a base, it is possible to improve the cooling efficiency by isolating elements by insulating properties that take advantage of the characteristics of wide bandgap and by high thermal conductivity.
  • FIG. 1 is a flowchart showing an example of a method for producing a heteroepitaxial film of the present invention
  • FIG. 5 is a graph showing an example of a growth sequence from the first step to the third step of the first embodiment
  • FIG. 2 is a flowchart showing an example of how a heteroepitaxial film is produced by peeling a 3C—SiC single crystal film from a single crystal silicon substrate.
  • FIG. 10 is a flowchart showing another example of how a heteroepitaxial film is produced by peeling a 3C—SiC single crystal film from a single crystal silicon substrate; 9 is a graph showing an example of a growth sequence in the first to third steps of the second embodiment; It is a graph which shows an example of the growth sequence from the 1st process of 3rd Embodiment to the 3rd process. 4 is a graph showing the results of in-plane XRD analysis of SiC on Si (111) grown in Example 1 (first embodiment).
  • 1 is a measurement diagram showing a cross-sectional TEM image of SiC-on-Si of Example 1 (first embodiment).
  • FIG. FIG. 10 is a measurement diagram showing a cross-sectional TEM image of SiC-on-Si of Example 2 (second embodiment).
  • second step SiC single crystals easily grow And, by combining predetermined conditions [pressure: 1333 Pa or less, temperature: 800 ° C. or more and less than 1200 ° C.] (third step) to form holes at the 3C-SiC / silicon interface, high-quality 3C- A SiC single crystal film can be efficiently formed, and furthermore, if the 3C-SiC single crystal film is separated from the single crystal silicon substrate by the vacancies and peeled off (fourth step), a heteroepitaxial film can be obtained efficiently. and completed the present invention.
  • FIG. 1 is a flowchart showing an example of the method for producing a heteroepitaxial film of the present invention.
  • the first step of hydrogen baking hereinafter also referred to as H 2 annealing
  • the second step of SiC nucleation step and the third step of SiC single crystal growth step (3C-SiC single crystal film formation step) , if necessary, a device process, a dicing process, and a fourth process of peeling off the heteroepitaxial film (3C-SiC single crystal film).
  • FIG. 2 shows an example of a growth sequence in the first to third steps of the first embodiment. Each step will be described below.
  • a single crystal silicon substrate is placed in a low pressure CVD apparatus (hereinafter also referred to as an RP-CVD apparatus), hydrogen gas is introduced, and a natural oxide film on the surface is removed by H 2 annealing. If the oxide film remains, SiC nucleation cannot be formed on the single crystal silicon substrate.
  • the H 2 annealing at this time is preferably carried out under the condition that the temperature is, for example, 1000° C. or more and 1200° C. or less. By setting the temperature to 1000° C.
  • H 2 annealing pressure and time are not particularly limited as long as the natural oxide film can be removed. In the example shown in FIG. 2, H 2 annealing is performed at 1080° C. for 1 minute.
  • hydrogen gas can be continuously introduced after the first step and also in the second and third steps (carrier gas).
  • the single crystal silicon substrate is set to a predetermined pressure and temperature, and a source gas containing carbon and silicon is introduced into the RP-CVD apparatus as a source gas for SiC to form SiC nuclei.
  • a source gas containing carbon and silicon is introduced into the RP-CVD apparatus as a source gas for SiC to form SiC nuclei.
  • monomethylsilane or trimethylsilane (TMS) can be introduced as the source gas. It is simpler and easier to control than the case of using multiple kinds of gases, and it is possible to form a 3C—SiC single crystal film more reliably.
  • TMS trimethylsilane
  • C atoms are smaller than Si and easily vaporize
  • trimethylsilane is easier to set conditions in consideration of raw material efficiency.
  • Such introduction of the source gas is performed in this second step and the following third step.
  • this SiC nucleation can be performed on the surface of the single crystal silicon substrate at a pressure of 1333 Pa (10 Torr) or less and a temperature of 300° C. or more and 950° C. or less.
  • the temperature is higher than 950° C., the reaction between the single crystal silicon substrate and the raw material gas proceeds, making it impossible to form SiC nuclei on the surface of the single crystal silicon substrate.
  • the temperature is less than 300° C., the temperature is too low to efficiently form SiC nuclei.
  • heteroepitaxial growth of SiC does not proceed if the temperature is lower than 800° C. in the third step.
  • the SiC nucleation temperature can be set to preferably 800° C. or higher and 950° C. or lower, more preferably 850° C. or higher and 900° C. or lower.
  • the SiC nucleation step (second step) and the subsequent third step of forming the 3C—SiC single crystal film should be set.
  • the temperature ranges can overlap, in particular these second and third steps can be carried out under the same temperature conditions.
  • the pressure is set to 1333 Pa (10 Torr) or less, it is possible to prevent the occurrence of secondary or higher-order reactions such as reaction of the reactive species with the raw material gas in the gas phase, which is efficient.
  • the lower limit of the pressure is not particularly limited, it can be set to 13 Pa (0.1 Torr), for example.
  • the pressure can be set to the same conditions in the second and third steps. In the example shown in FIG. 2, the second step and the following third step are performed under the same conditions, the same pressure, and the same holding temperature (900° C.).
  • the 3C—SiC single crystal film forming step which is the third step, is performed under the conditions of a pressure of 1333 Pa (10 Torr) or less and a temperature of 800° C. or more and less than 1200° C. Under such conditions, the SiC single crystal can be efficiently grown to form the 3C-SiC single crystal film.
  • the pressure is set to 1333 Pa (10 Torr) or less in the third step, polycrystallization of the 3C-SiC to be formed can be prevented. Furthermore, higher-order reactions can be suppressed, and a 3C—SiC single crystal film can be reliably and efficiently formed.
  • the lower limit of the pressure is not particularly limited, it can be set to 13 Pa (0.1 Torr), for example.
  • the temperature if the temperature is less than 800° C., the growth of the SiC single crystal does not proceed as described above, and if it is 1200° C. or more, slip dislocations may occur. Therefore, the temperature is set to 800° C. or more and less than 1200° C. as described above. In the example shown in FIG. 2, the second and third steps are performed under the same conditions as described above, and SiC nucleation and 3C—SiC single crystal film formation are continuously performed.
  • the film formation time can be appropriately set based on the pressure and temperature conditions set so as to obtain the desired film thickness.
  • the thickness of the 3C-SiC single crystal film can range from a thin film of about 2 nm to a thick film of several ⁇ m.
  • layered growth in the two-dimensional growth mode shown in FIG. 2 is layer-by-layer epitaxial growth.
  • GaN is grown by MOCVD using organometallic materials such as trimethylgallium and trimethylammonium to grow GaN to a thickness of about 3 ⁇ m.
  • this 3C--SiC single crystal film becomes a withstand voltage holding layer in the IGBT.
  • the dielectric breakdown field strength of silicon is 0.3 MV/cm
  • the dielectric breakdown field strength of 3C-SiC is 3 MV/cm, which is 10 times greater than that of 3C-SiC. That is, equivalent performance can be obtained with a thickness of 1/10 of the thickness of the breakdown voltage holding layer of the conventional silicon IGBT.
  • the breakdown voltage holding layer only with the 3C-SiC single crystal film, and a combination of SiC and Si is sufficient.
  • a Si epitaxial layer is grown on the SiC grown to a predetermined thickness in this manner.
  • the gate insulating film is formed using SiC, and there was a reliability problem. , it becomes possible to ensure the same gate reliability as the conventional silicon IGBT.
  • the thickness of the silicon layer at this time may be set arbitrarily as long as it is thicker than the required gate structure.
  • FIG. 3 shows an example of how a heteroepitaxial film is produced by peeling a 3C—SiC single crystal film from a single crystal silicon substrate.
  • the heteroepitaxial film 3 is formed on the single crystal silicon substrate 1 by the steps up to this point.
  • the heteroepitaxial film 3 contains at least a 3C-SiC single crystal film. , a case of having a 3C—SiC film and a Si film in order from the single crystal silicon substrate side.
  • a vacancy region 2 (3C - is a region in which vacancies are formed at the SiC/silicon interface, and is also referred to as a vacancy forming portion) is formed.
  • a protective film 4 is formed on the 3C—SiC single crystal film (in other words, on the surface of the heteroepitaxial film 3).
  • the material of the protective film 4 include resin such as polyimide and an oxide film deposited by CVD.
  • FIG. 4 shows another example of how a heteroepitaxial film is produced.
  • a device is formed on the 3C—SiC single crystal film (on the surface of the heteroepitaxial film 3) ( ⁇ device process> in FIG. 1: heteroepitaxial film 3′ after device formation), for example, a dicing machine. 5 ( ⁇ dicing step> in FIG. 1), and in the fourth step, the heteroepitaxial film 3′ is separated at the hole region 2 and peeled off.
  • the heteroepitaxial film 3' obtained by peeling is chip-shaped (chip 6).
  • a clipper, a picker, or the like can be used for the peeling, and the single-crystal silicon substrate 1 can be easily removed with these. After that, it can be attached to another wafer or a substrate made of a different material to fabricate an element. Note that scribing can also be performed instead of dicing.
  • the fourth step may be performed after forming a protective film.
  • a device may be formed on the 3C—SiC single crystal film, the device may be cut out along the scribe lines of the device, and then the protective film may be formed before performing the fourth step.
  • the fourth step can also be performed after adhering to a holding base (for example, various substrates) with an adhesive with or without a protective film. In this manner, necessary treatments can be appropriately performed between the third step and the fourth step depending on the form of the desired heteroepitaxial film.
  • heteroepitaxial film manufacturing method of the present invention it is possible to efficiently form a heteroepitaxial film with holes, and even if a device has already been formed by separation and separation in the hole region, A heteroepitaxial film can be obtained efficiently and simply with little damage to the device. Moreover, since the 3C-SiC single crystal film and the single crystal silicon substrate can be separated at the interface, the loss of the single crystal silicon substrate obtained after the separation can be greatly reduced, and can be reused for the production of the next heteroepitaxial film. can be done.
  • FIG. 5 shows an example of the growth sequence in the first to third steps of the second embodiment.
  • the single crystal silicon substrate is set to a temperature of 300° C. or higher and 950° C. or lower, preferably 800° C. or higher and 950° C. or lower, more preferably 850° C. or higher and 900° C. or lower. Introduce monomethylsilane or trimethylsilane. Nucleation time can be, for example, 5 minutes.
  • ⁇ Third step> As a step of forming a 3C—SiC single crystal film, the single crystal silicon substrate is heated to a temperature of 1000° C. or more and less than 1200° C., and monomethylsilane or trimethylsilane is introduced as a source gas for SiC.
  • the third step which is the step of forming the 3C—SiC single crystal film
  • high-speed growth is facilitated (between steps change in ).
  • High-speed growth can also be facilitated by increasing one or more of the pressure and temperature during the third step (change during the step). Either one of the above inter-process and intra-process changes may be made, or both may be made.
  • the temperature in the third step can be set to 1000°C or higher and lower than 1200°C. In this case, heteroepitaxial growth can be rate-limiting for feed gas transport. It is not subject to the restrictions of the plane orientation of the single-crystal silicon substrate, and can easily deal with large-diameter substrates such as 300 mm in diameter.
  • FIG. 5 shows an example in which only changes are made between steps, in which the second step is held at 900° C., and the third step is held at 1190° C. (the pressure is, for example, same for ).
  • the pressure is, for example, same for .
  • the introduction of trimethylsilane is resumed in the third step to 900 ° C., or It is also possible to raise the temperature to 1190° C. and hold it after maintaining the temperature above 900° C. and below 1190° C. for a predetermined period of time.
  • the growth is performed at a higher temperature (1190° C.) than in the first embodiment (900° C.). 2 is flowing, the effect of H2 , or the effect of changing the growth mode by changing the temperature during the growth (that is, when moving from the second step to the third step). can be considered.
  • the sequence of FIG. 5 also proceeds from nucleation to two-dimensional growth.
  • the pressure is set to 1333 Pa (10 Torr) or less, preferably 133 Pa (1 Torr) or less to form vacancies directly under the 3C-SiC single crystal film. Then, by changing the pressure to a condition higher than the initial stage within the range of 1333 Pa (10 Torr) or less, it is possible to achieve both relaxation of the stress in the entire heteroepitaxial layer and efficient formation of the 3C-SiC single crystal film. can be done.
  • a heteroepitaxial film is produced by separating the formed 3C—SiC single crystal film from the single crystal silicon substrate by vacancies. It can be performed in the same manner as in the first embodiment.
  • FIG. 6 shows an example of the growth sequence of the third embodiment.
  • ⁇ Second step, third step> in order to continuously form SiC nuclei on the surface of the single crystal silicon substrate and subsequently form a 3C—SiC single crystal film, the temperature is maintained at 300° C. or more and 950° C. or less while introducing monomethylsilane or trimethylsilane as a raw material gas. to a temperature in the range of 1000°C or higher and lower than 1200°C. In this manner, the second step and the third step can be performed continuously while the temperature is being raised. It is preferable that the heating rate is, for example, 0.5° C./sec or more and 2° C./sec or less.
  • This level of temperature increase rate is not too high, so it is possible to effectively prevent deviation between the set temperature and the actual temperature, and the temperature can be appropriately controlled.
  • the heating rate is not too slow, it is possible to suppress the increase in transit time of the nucleation temperature zone of SiC, which tends to cause non-uniform nucleation, and the tendency for defect formation during heteroepitaxial growth to occur. .
  • the growth may be stopped there, or the temperature may be maintained until the predetermined film thickness is reached. May continue to grow. Alternatively, even if the temperature reaches 1000° C. or higher but does not reach the predetermined temperature, the growth may be stopped when the predetermined film thickness is reached during the temperature rise.
  • the temperature is raised from 300° C. to 1130° C. at a temperature elevation rate of 1° C./sec and maintained at 1130° C. for a predetermined time.
  • the pressure is set to 1333 Pa (10 Torr) or less, preferably 133 Pa (1 Torr) or less to form vacancies directly under the 3C-SiC single crystal film. Then, by changing the pressure to a condition higher than the initial stage within the range of 1333 Pa (10 Torr) or less, it is possible to achieve both relaxation of the stress in the entire heteroepitaxial layer and efficient formation of the 3C-SiC single crystal film. can be done.
  • a heteroepitaxial film is produced by separating the formed 3C—SiC single crystal film from the single crystal silicon substrate by vacancies. It can be performed in the same manner as in the first embodiment.
  • Example 1 A 300 mm diameter, (111) plane orientation, boron-doped high resistivity single crystal silicon substrate was prepared, the wafer was placed on a susceptor in a reactor of an RP-CVD apparatus, and H 2 annealing was performed at 1080° C. for 1 minute. (first step). Subsequently, trimethylsilane gas was introduced at a growth temperature of 900° C. and a growth pressure of 133 Pa (1 Torr), and a SiC nucleation step (second step) and a 3C—SiC single crystal film were grown (third step). . As a result of growing for 5 minutes, the film thickness was 13 nm.
  • the 3C-SiC single crystal film (heteroepitaxial film) could be separated and peeled from the vacancy formation part at the 3C-SiC/silicon interface ( fourth step).
  • the substrate on which the 3C-SiC single crystal film is grown is diced from the 3C-SiC single crystal film side to a size of 1 mm ⁇ 1 mm (the dicing depth is 3C-SiC single crystal film). It was slightly deeper than the thickness of the crystal film), and the 3C—SiC single crystal film could be peeled off at the hole forming portion as a chip by sucking the surface with a clipper.
  • Example 2 A boron-doped high-resistivity single-crystal silicon substrate with a diameter of 300 mm and a plane orientation of (111) was prepared. (First step). Subsequently, trimethylsilane gas was introduced for 5 minutes at a growth temperature of 900° C. as a second step (nucleation step of SiC nuclei). Next, in the third step (3C-SiC single crystal film forming step), the growth temperature was raised to 1190° C. and trimethylsilane gas was introduced to grow a 3C-SiC single crystal film. The growth pressure at this time was uniformly 133 Pa (1 Torr). As a result of growing for 1 minute, the film thickness was about 30 nm.
  • Example 3 A 3C—SiC single crystal film was formed under the same conditions as in Example 1 except that the growth pressure in the second and third steps was 1333 Pa (10 Torr) and the growth temperature was 950°C. As a result, the film thickness was about 20 nm. After that, when the XRD spectrum was confirmed in the In Plane arrangement, a peak of 3C-SiC (220) parallel to Si (220) could be confirmed, and it was confirmed that a single crystal 3C-SiC film was growing. confirmed. Also, it was confirmed that vacancies were formed directly under the 3C—SiC single crystal film. Furthermore, when the fourth step was performed in the same manner as in Example 1 using an adhesive and a quartz substrate, the 3C-SiC single crystal film could be peeled off from the vacancy formation portion at the 3C-SiC/silicon interface. rice field.
  • Example 4 A 3C—SiC single crystal film was formed under the same conditions as in Example 2 except that the growth temperatures in the second and third steps were 300° C. and 800° C., respectively. As a result, the film thickness was about 12 nm. After that, when the XRD spectrum was confirmed in the In Plane arrangement, a peak of 3C-SiC (220) parallel to Si (220) could be confirmed, and it was confirmed that a single crystal 3C-SiC film was growing. confirmed. Also, it was confirmed that vacancies were formed directly under the 3C—SiC single crystal film. Furthermore, when the fourth step was performed in the same manner as in Example 2 using an adhesive and a quartz substrate, the 3C-SiC single crystal film could be peeled off from the hole formation portion at the 3C-SiC/silicon interface. rice field.
  • Example 1 A 3C—SiC single crystal film was formed under the same conditions as in Example 2 except that the growth pressure in the second and third steps was 3999 Pa (30 Torr). As a result, the film thickness was about 33 nm. After that, when the XRD spectrum was confirmed in the In Plane arrangement, a peak of 3C-SiC (220) parallel to Si (220) could be confirmed, and it was confirmed that a single crystal 3C-SiC film was growing. confirmed. However, formation of vacancies directly below the 3C--SiC single crystal film could not be confirmed. Furthermore, an attempt was made to separate the 3C-SiC single crystal film using an adhesive and a quartz substrate in the same manner as in Example 2, but the separation could not be achieved. It is considered that this is because the above-mentioned voids could not be formed.
  • Example 2 A 3C—SiC single crystal film was formed under the same conditions as in Example 2 except that the growth temperature in the second step was set to 200°C or 1000°C. As a result, the film thicknesses were approximately 2 nm and 4 nm, respectively. The film thickness formed in this way was extremely thin compared to Example 2, and the efficiency was extremely poor. This is probably because SiC was not sufficiently nucleated because the temperature in the second step was either too low or too high, and therefore heteroepitaxial growth hardly occurred in the third step.
  • Example 3 A 3C—SiC single crystal film was formed under the same conditions as in Example 2, except that the growth temperature in the third step was set to 700°C or 1250°C. As a result, the film thicknesses were about 7 nm and 50 nm, respectively. Thus, in the case of 700° C., the formed film thickness was extremely thin as compared with that of Example 2, and the efficiency was extremely poor. Moreover, in the case of 1250° C., slip dislocation occurred.
  • the present invention is not limited to the above embodiments.
  • the above embodiment is an example, and any device that has substantially the same configuration as the technical idea described in the claims of the present invention and produces similar effects is the present invention. It is included in the technical scope of the invention.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Inorganic Chemistry (AREA)
  • Mechanical Engineering (AREA)
  • Crystals, And After-Treatments Of Crystals (AREA)
  • Chemical Vapour Deposition (AREA)
PCT/JP2022/032016 2021-10-06 2022-08-25 ヘテロエピタキシャル膜の作製方法 Ceased WO2023058355A1 (ja)

Priority Applications (5)

Application Number Priority Date Filing Date Title
CN202280067121.0A CN118176329A (zh) 2021-10-06 2022-08-25 异质外延膜的制作方法
US18/695,073 US20250163609A1 (en) 2021-10-06 2022-08-25 Method for producing heteroepitaxial film
EP22878226.4A EP4414483B1 (en) 2021-10-06 2022-08-25 Method for forming heteroepitaxial film
JP2023552739A JP7708198B2 (ja) 2021-10-06 2022-08-25 ヘテロエピタキシャル膜の作製方法
KR1020247010927A KR102957204B1 (ko) 2021-10-06 2022-08-25 헤테로에피택셜막의 제작방법

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021164648 2021-10-06
JP2021-164648 2021-10-06

Publications (1)

Publication Number Publication Date
WO2023058355A1 true WO2023058355A1 (ja) 2023-04-13

Family

ID=85803388

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/032016 Ceased WO2023058355A1 (ja) 2021-10-06 2022-08-25 ヘテロエピタキシャル膜の作製方法

Country Status (7)

Country Link
US (1) US20250163609A1 (cg-RX-API-DMAC7.html)
EP (1) EP4414483B1 (cg-RX-API-DMAC7.html)
JP (1) JP7708198B2 (cg-RX-API-DMAC7.html)
KR (1) KR102957204B1 (cg-RX-API-DMAC7.html)
CN (1) CN118176329A (cg-RX-API-DMAC7.html)
TW (1) TW202321507A (cg-RX-API-DMAC7.html)
WO (1) WO2023058355A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026163721A1 (ja) * 2025-01-29 2026-08-06 信越半導体株式会社 半導体基板及びその製造方法

Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2006036609A (ja) * 2004-07-29 2006-02-09 Fuji Electric Holdings Co Ltd 炭化珪素半導体基板の製造方法
JP2010502023A (ja) 2006-08-30 2010-01-21 ジルトロニック アクチエンゲゼルシャフト 多層半導体ウエハ及びその製造方法
JP2010251724A (ja) 2009-03-26 2010-11-04 Semiconductor Energy Lab Co Ltd 半導体基板の作製方法
JP2011071219A (ja) * 2009-09-24 2011-04-07 Seiko Epson Corp 半導体基板の製造方法
JP2011223011A (ja) 2002-11-07 2011-11-04 Commiss Energ Atom 同時注入により基板内に脆性領域を生成する方法
JP2014237581A (ja) * 2014-07-01 2014-12-18 セイコーエプソン株式会社 立方晶炭化珪素半導体基板
JP2018070435A (ja) * 2016-11-04 2018-05-10 セイコーエプソン株式会社 半導体基板の製造方法

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3557457B2 (ja) * 2001-02-01 2004-08-25 東北大学長 SiC膜の製造方法、及びSiC多層膜構造の製造方法
JP4353369B2 (ja) * 2004-06-07 2009-10-28 コバレントマテリアル株式会社 SiC半導体及びその製造方法
JP2006253617A (ja) * 2005-02-14 2006-09-21 Toshiba Ceramics Co Ltd SiC半導体およびその製造方法

Patent Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2011223011A (ja) 2002-11-07 2011-11-04 Commiss Energ Atom 同時注入により基板内に脆性領域を生成する方法
JP2006036609A (ja) * 2004-07-29 2006-02-09 Fuji Electric Holdings Co Ltd 炭化珪素半導体基板の製造方法
JP2010502023A (ja) 2006-08-30 2010-01-21 ジルトロニック アクチエンゲゼルシャフト 多層半導体ウエハ及びその製造方法
JP2010251724A (ja) 2009-03-26 2010-11-04 Semiconductor Energy Lab Co Ltd 半導体基板の作製方法
JP2011071219A (ja) * 2009-09-24 2011-04-07 Seiko Epson Corp 半導体基板の製造方法
JP2014237581A (ja) * 2014-07-01 2014-12-18 セイコーエプソン株式会社 立方晶炭化珪素半導体基板
JP2018070435A (ja) * 2016-11-04 2018-05-10 セイコーエプソン株式会社 半導体基板の製造方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4414483A4

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026163721A1 (ja) * 2025-01-29 2026-08-06 信越半導体株式会社 半導体基板及びその製造方法

Also Published As

Publication number Publication date
EP4414483A1 (en) 2024-08-14
JP7708198B2 (ja) 2025-07-15
EP4414483B1 (en) 2026-07-22
KR20240088776A (ko) 2024-06-20
JPWO2023058355A1 (cg-RX-API-DMAC7.html) 2023-04-13
EP4414483A4 (en) 2025-08-20
KR102957204B1 (ko) 2026-04-24
CN118176329A (zh) 2024-06-11
US20250163609A1 (en) 2025-05-22
TW202321507A (zh) 2023-06-01

Similar Documents

Publication Publication Date Title
TWI736554B (zh) SiC複合基板之製造方法
JP5498163B2 (ja) 多層半導体ウエハ及びその製造方法並びに素子
CN112262456B (zh) GaN层叠基板的制造方法
JP7259906B2 (ja) ヘテロエピタキシャルウェーハの製造方法
CN104584190B (zh) 外延晶片及其制造方法
US9099308B2 (en) Semiconductor wafer and method for manufacturing the same
TWI873372B (zh) 製作用於磊晶生長基於鎵之iii族氮化物合金層之底材之方法
EP2602812A1 (en) High-quality gan high-voltage hfets on silicon
JP7708198B2 (ja) ヘテロエピタキシャル膜の作製方法
JP6763347B2 (ja) 窒化物半導体基板の製造方法および窒化物半導体基板
KR100288473B1 (ko) 단결정탄화규소 및 그 제조방법
JP7218832B1 (ja) ヘテロエピタキシャルウェーハの製造方法
CN119252732A (zh) 一种硅衬底氮化镓半导体晶片及其制备方法和应用
KR20250069864A (ko) 질화물 반도체층 부착 단결정 실리콘기판 및 질화물 반도체층 부착 단결정 실리콘기판의 제조방법
CN118215987A (zh) 氮化物半导体基板及氮化物半导体基板的制造方法
JP7810099B2 (ja) ヘテロエピタキシャル基板の製造方法
EP4729669A1 (en) Method for manufacturing sic substrate, method for manufacturing semiconductor device, sic substrate, and semiconductor device
JP2024543550A (ja) 多結晶シリコンカーバイド基板と単結晶シリコンカーバイドの活性層とを備える半導体構造の製造のためのプロセス
CN121204818A (zh) 一种硅掺氮化镓晶碇及其生长方法
CN119730282A (zh) 复合衬底及其制备方法、半导体结构、电子设备

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22878226

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2023552739

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 18695073

Country of ref document: US

WWE Wipo information: entry into national phase

Ref document number: 202280067121.0

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 2022878226

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2022878226

Country of ref document: EP

Effective date: 20240506

WWP Wipo information: published in national office

Ref document number: 18695073

Country of ref document: US

WWG Wipo information: grant in national office

Ref document number: 2022878226