WO2021006314A1 - Procédé de fabrication de corps de rouleau, et corps de rouleau - Google Patents

Procédé de fabrication de corps de rouleau, et corps de rouleau Download PDF

Info

Publication number
WO2021006314A1
WO2021006314A1 PCT/JP2020/026863 JP2020026863W WO2021006314A1 WO 2021006314 A1 WO2021006314 A1 WO 2021006314A1 JP 2020026863 W JP2020026863 W JP 2020026863W WO 2021006314 A1 WO2021006314 A1 WO 2021006314A1
Authority
WO
WIPO (PCT)
Prior art keywords
sheet
winding core
roll body
gap
winding
Prior art date
Application number
PCT/JP2020/026863
Other languages
English (en)
Japanese (ja)
Inventor
将宏 鳥本
恵 大石
亮 秋山
遼 中澤
博大 馬橋
章 谷口
橋本 浩二
隆介 長町
雅允 中野
勇二 大原
Original Assignee
大日本印刷株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 大日本印刷株式会社 filed Critical 大日本印刷株式会社
Priority to CN202080054223.XA priority Critical patent/CN114223081A/zh
Priority to KR1020227003825A priority patent/KR20220029738A/ko
Publication of WO2021006314A1 publication Critical patent/WO2021006314A1/fr

Abstract

L'invention concerne : un procédé de fabrication d'un corps de rouleau, ledit procédé permettant de réduire efficacement une différence de niveau provoquée au niveau d'une extrémité de début d'enroulement d'une feuille ; et ledit corps de rouleau. Un aspect de la présente invention concerne un procédé de fabrication d'un corps de rouleau 10 comprenant un noyau d'enroulement 11 et une feuille allongée 12 qui est enroulée autour d'une surface circonférentielle externe 11A du noyau d'enroulement 11, ledit procédé comprenant : une étape pour appliquer un matériau de revêtement 18 sur la surface circonférentielle externe 11A du noyau d'enroulement 11 le long d'une direction de largeur DR1 du noyau d'enroulement 11 ; une étape pour placer, sur la surface circonférentielle externe 11A, une extrémité de début d'enroulement 12A dans une direction longitudinale DR2 de la feuille 12 ; et une étape pour enrouler la feuille 12 autour du noyau d'enroulement 11 et remplir au moins un premier espace 13 avec le matériau de revêtement 18. L'application du matériau de revêtement 18 ou le placement de l'extrémité de début d'enroulement 12A est effectué de telle sorte que le matériau de revêtement 18 entre en contact avec, ou est à proximité de, une surface d'extrémité distale 12A1 située dans la direction longitudinale DR2 de l'extrémité de début d'enroulement 12A, et le premier espace 13 est situé entre le noyau d'enroulement 11 et le premier enroulement de la feuille 12 et est en contact avec la surface d'extrémité distale 12A1.
PCT/JP2020/026863 2019-07-09 2020-07-09 Procédé de fabrication de corps de rouleau, et corps de rouleau WO2021006314A1 (fr)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN202080054223.XA CN114223081A (zh) 2019-07-09 2020-07-09 卷体的制造方法和卷体
KR1020227003825A KR20220029738A (ko) 2019-07-09 2020-07-09 롤체의 제조 방법 및 롤체

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP2019127551 2019-07-09
JP2019-127551 2019-07-09
JP2020007594 2020-01-21
JP2020-007594 2020-01-21

Publications (1)

Publication Number Publication Date
WO2021006314A1 true WO2021006314A1 (fr) 2021-01-14

Family

ID=74114519

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2020/026863 WO2021006314A1 (fr) 2019-07-09 2020-07-09 Procédé de fabrication de corps de rouleau, et corps de rouleau

Country Status (5)

Country Link
JP (1) JP2021107286A (fr)
KR (1) KR20220029738A (fr)
CN (1) CN114223081A (fr)
TW (1) TW202108488A (fr)
WO (1) WO2021006314A1 (fr)

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2011201634A (ja) * 2010-03-25 2011-10-13 Maxell Sliontec Ltd ロール状物の段差痕低減構造及びロール状物の製造方法
JP2016155619A (ja) * 2015-02-23 2016-09-01 プロマティック株式会社 ロール材料およびその製造方法

Family Cites Families (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005075521A (ja) 2003-08-29 2005-03-24 Murazumi Kk 巻芯及び該巻芯を用いたロール状物
JP5088567B2 (ja) * 2008-03-31 2012-12-05 東レフィルム加工株式会社 ウェブ状物巻取り用巻芯およびウェブ状物巻き取り方法
JP5623453B2 (ja) 2012-03-26 2014-11-12 富士フイルム株式会社 ポリマーフィルムロール、光学フィルム及びポリマーフィルムロール製造方法
JP2014151985A (ja) * 2013-02-05 2014-08-25 Dainippon Printing Co Ltd 巻芯および巻体
JPWO2014178393A1 (ja) * 2013-05-02 2017-02-23 日本発條株式会社 フィルム巻取り用コア
JP6472077B2 (ja) * 2015-03-23 2019-02-20 グラフテック株式会社 ロール紙幅規制鍔及びそれを有する印刷システム
CN205177930U (zh) * 2015-12-17 2016-04-20 吉安力莱新能源科技有限公司 防短路电池

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2011201634A (ja) * 2010-03-25 2011-10-13 Maxell Sliontec Ltd ロール状物の段差痕低減構造及びロール状物の製造方法
JP2016155619A (ja) * 2015-02-23 2016-09-01 プロマティック株式会社 ロール材料およびその製造方法

Also Published As

Publication number Publication date
TW202108488A (zh) 2021-03-01
JP2021107286A (ja) 2021-07-29
CN114223081A (zh) 2022-03-22
KR20220029738A (ko) 2022-03-08

Similar Documents

Publication Publication Date Title
TWI528056B (zh) 偏光板的製造方法
JP6852967B2 (ja) 粘着剤層付偏光フィルム、光学部材、及び画像表示装置
KR102004172B1 (ko) 이방 점착성 시트
WO2009087942A1 (fr) Polarisateur
JP2012144690A (ja) 活性エネルギー線硬化型接着剤組成物、偏光板、光学フィルムおよび画像表示装置
TWI569048B (zh) Method for manufacturing optical members with adhesive
WO2018221232A1 (fr) Film optique, procédé de pelage et procédé de fabrication de panneau d'affichage optique
US9932500B2 (en) Adhesive tape
US20220184937A1 (en) Transfer sheet and manufacturing method for same, method for manufacturing molded body using said transfer sheet and molded body, and front plate using said molded body and image display device
JP2015508339A (ja) 光学的に透明なフィルムのための変性剥離コーティング
WO2021006314A1 (fr) Procédé de fabrication de corps de rouleau, et corps de rouleau
JP6872485B2 (ja) マイクロスフェア処理した縁部を有するウェブ巻取りロール及びその作製方法
JP2003027019A (ja) 光学シート保護用粘着フィルム
JP2004029204A (ja) 光学シート保護用粘着フィルム
WO2022025289A1 (fr) Corps de rouleau
JP5089144B2 (ja) ラビング布貼付け用両面粘着テープ及びそれを貼着してなるローラ
JP2015199265A (ja) 基材レス両面粘着シート用離型フィルム
JP2013237849A (ja) 活性エネルギー線硬化型接着剤組成物、偏光板、光学フィルムおよび画像表示装置
JP7258497B2 (ja) 透明粘着フィルム
JP2002173650A (ja) 光学シート保護用粘着フィルム
JP7154002B2 (ja) 偏光フィルム、粘着剤層付き偏光フィルム、及び画像表示装置
WO2017138449A1 (fr) Procédé de fabrication de film optique stratifié
JP2020052170A (ja) 光学積層体
JP2020033441A (ja) 両面粘着テープ
WO2019065874A1 (fr) Film adhésif transparent

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 20837504

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 20227003825

Country of ref document: KR

Kind code of ref document: A

122 Ep: pct application non-entry in european phase

Ref document number: 20837504

Country of ref document: EP

Kind code of ref document: A1