WO2005061648A1 - Composition adhesive autocollante destinee a un film optique, couche adhesive autocollante destinee a un film optique, film optique de type adhesif autocollant et affichage d'images - Google Patents

Composition adhesive autocollante destinee a un film optique, couche adhesive autocollante destinee a un film optique, film optique de type adhesif autocollant et affichage d'images Download PDF

Info

Publication number
WO2005061648A1
WO2005061648A1 PCT/JP2004/017871 JP2004017871W WO2005061648A1 WO 2005061648 A1 WO2005061648 A1 WO 2005061648A1 JP 2004017871 W JP2004017871 W JP 2004017871W WO 2005061648 A1 WO2005061648 A1 WO 2005061648A1
Authority
WO
WIPO (PCT)
Prior art keywords
optical film
sensitive adhesive
pressure
film
polymer
Prior art date
Application number
PCT/JP2004/017871
Other languages
English (en)
Japanese (ja)
Inventor
Yuusuke Toyama
Masayuki Satake
Akiko Ogasawara
Fumiaki Shirafuji
Original Assignee
Nitto Denko Corporation
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Denko Corporation filed Critical Nitto Denko Corporation
Publication of WO2005061648A1 publication Critical patent/WO2005061648A1/fr

Abstract

L'invention concerne une composition adhésive autocollante destinée à des films optiques et inhibant de manière efficace une fuite de rayonnement et une inégalité de motif de cadre de fenêtre même dans des conditions de température élevée d'environ 120 °C. La composition adhésive autocollante destinée à des films optiques comprend: un polymère (méth)acrylate possédant un poids moléculaire moyen en poids compris entre 500'00 et 2'500'00; un oligomère (méth)acrylate possédant un poids moléculaire moyen en poids compris entre 1,000 et 10,000 obtenu par polymérisation avec un agent de migration de chaîne comprenant une double liaison réactive carbone-carbone; et un agent de réticulation. Cette composition est caractérisée en ce que la teneur de l'agent de migration de chaîne dans la composition est d'au plus 0,3 en termes de rapport d'absorbance [(absorbance attribuable à la vibration C=C dans l'agent de migration de chaîne dans une région de 780±20 cm-1)/(absorbance attribuable à la vibration C-H dans les polymère et oligomère dans une région de 740±20 cm-1)&rsqb
PCT/JP2004/017871 2003-12-18 2004-12-01 Composition adhesive autocollante destinee a un film optique, couche adhesive autocollante destinee a un film optique, film optique de type adhesif autocollant et affichage d'images WO2005061648A1 (fr)

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2003-420993 2003-12-18
JP2003420993A JP2005179467A (ja) 2003-12-18 2003-12-18 光学フィルム用粘着剤組成物、光学フィルム用粘着剤層、粘着型光学フィルムおよび画像表示装置

Publications (1)

Publication Number Publication Date
WO2005061648A1 true WO2005061648A1 (fr) 2005-07-07

Family

ID=34708711

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2004/017871 WO2005061648A1 (fr) 2003-12-18 2004-12-01 Composition adhesive autocollante destinee a un film optique, couche adhesive autocollante destinee a un film optique, film optique de type adhesif autocollant et affichage d'images

Country Status (3)

Country Link
JP (1) JP2005179467A (fr)
TW (1) TW200531828A (fr)
WO (1) WO2005061648A1 (fr)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2009507255A (ja) * 2005-09-05 2009-02-19 エルジー・ケム・リミテッド 偏光板用アクリル系粘着剤組成物

Families Citing this family (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP1931744B1 (fr) 2005-09-05 2016-05-04 LG Chem, Ltd. Composition acrylique adhesive sensible a la pression pour la polarisation d'un film
JP4673344B2 (ja) * 2007-06-07 2011-04-20 日東電工株式会社 光学フィルム用粘着シートの製造方法
JP2011090312A (ja) * 2010-11-09 2011-05-06 Nitto Denko Corp 画像表示装置の光学フィルム用粘着シート、粘着型光学フィルムおよび画像表示装置
JP5968175B2 (ja) * 2012-09-20 2016-08-10 リンテック株式会社 電子部品用両面粘着シート
JP6122337B2 (ja) 2013-04-26 2017-04-26 日東電工株式会社 偏光フィルムおよびその製造方法、光学フィルムおよび画像表示装置
JP2015205974A (ja) * 2014-04-18 2015-11-19 綜研化学株式会社 偏光板用粘着剤組成物、粘着シート、粘着剤層付き偏光板および積層体

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH10279907A (ja) * 1997-04-09 1998-10-20 Soken Chem & Eng Co Ltd 偏光板用粘着剤組成物および偏光板
JP2000109771A (ja) * 1998-10-07 2000-04-18 Lintec Corp 粘着シート
JP2001335767A (ja) * 2000-05-30 2001-12-04 Lintec Corp 粘着剤組成物、それを用いた粘着シート及び粘着性光学部材
JP2002030264A (ja) * 2000-07-18 2002-01-31 Lintec Corp 粘着剤組成物及びそれを用いた粘着性光学部材
JP2002121521A (ja) * 2000-10-13 2002-04-26 Nippon Carbide Ind Co Inc 偏光フィルム用粘着剤組成物及び偏光フィルム
JP2003049143A (ja) * 2001-05-31 2003-02-21 Soken Chem & Eng Co Ltd 光学フィルム用粘着剤及び該粘着剤を用いた光学フィルム

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH10279907A (ja) * 1997-04-09 1998-10-20 Soken Chem & Eng Co Ltd 偏光板用粘着剤組成物および偏光板
JP2000109771A (ja) * 1998-10-07 2000-04-18 Lintec Corp 粘着シート
JP2001335767A (ja) * 2000-05-30 2001-12-04 Lintec Corp 粘着剤組成物、それを用いた粘着シート及び粘着性光学部材
JP2002030264A (ja) * 2000-07-18 2002-01-31 Lintec Corp 粘着剤組成物及びそれを用いた粘着性光学部材
JP2002121521A (ja) * 2000-10-13 2002-04-26 Nippon Carbide Ind Co Inc 偏光フィルム用粘着剤組成物及び偏光フィルム
JP2003049143A (ja) * 2001-05-31 2003-02-21 Soken Chem & Eng Co Ltd 光学フィルム用粘着剤及び該粘着剤を用いた光学フィルム

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2009507255A (ja) * 2005-09-05 2009-02-19 エルジー・ケム・リミテッド 偏光板用アクリル系粘着剤組成物

Also Published As

Publication number Publication date
TW200531828A (en) 2005-10-01
JP2005179467A (ja) 2005-07-07

Similar Documents

Publication Publication Date Title
JP4805240B2 (ja) 粘着型光学フィルムおよび画像表示装置
JP3916638B2 (ja) 粘着型光学フィルムおよび画像表示装置
JP4800722B2 (ja) 光学用粘着剤組成物、光学用粘着剤層、粘着剤層付光学部材、その製造方法および画像表示装置
JP4780766B2 (ja) 光学用粘着剤、粘着剤付き光学フィルムおよび画像表示装置
KR100959048B1 (ko) 점착형 광학보상층을 갖는 편광판 및 화상표시장치
JP4800673B2 (ja) 粘着剤組成物、粘着剤層、粘着部材、粘着型光学部材および画像表示装置
WO2003107049A1 (fr) Plaque de polarisation munie d'une couche de compensation optique et dispositif d'affichage d'images
US8372492B2 (en) Pressure-sensitive adhesive optical film and image display
JP4780647B2 (ja) 光学フィルム用粘着剤、光学フィルム用粘着剤層およびその製造方法、粘着型光学フィルム、ならびに画像表示装置
JP5694972B2 (ja) 光学フィルム用粘着剤、光学フィルム用粘着剤層、粘着型光学フィルムおよび画像表示装置
JP2003329838A (ja) 粘着型光学フィルム、光学フィルム用粘着剤組成物および画像表示装置
JP4215124B2 (ja) 光学部材用粘着剤組成物、光学部材用粘着剤層、粘着型光学部材及びその製造方法、並びに画像表示装置
JP2003307624A (ja) 粘着型光学フィルムおよび画像表示装置
JP2004323543A (ja) 光学部材用粘着剤組成物、光学部材用粘着剤層、粘着型光学部材および画像表示装置
JP4727238B2 (ja) 光学部材用粘着剤組成物、光学部材用粘着剤層、粘着型光学部材、及び画像表示装置
JP4849625B2 (ja) 光学フィルム用粘着剤層の製造方法および粘着型光学フィルムの製造方法
JP4798752B2 (ja) 光学用粘着剤、粘着剤付き光学フィルムおよび画像表示装置
JP2003327926A (ja) 粘着型光学フィルム、光学フィルム用粘着剤組成物および画像表示装置
WO2005061648A1 (fr) Composition adhesive autocollante destinee a un film optique, couche adhesive autocollante destinee a un film optique, film optique de type adhesif autocollant et affichage d'images
JP2005048003A (ja) 光学部材用粘着剤組成物、光学部材用粘着剤層、粘着型光学部材及びその製造方法、画像表示装置、並びに粘着型光学部材の製造方法
JP2009008859A (ja) 粘着型光学フィルムおよび画像表示装置
TWI384043B (zh) An adhesive composition, a method for producing the same, and a use thereof
JP5202795B2 (ja) 光学部材用粘着剤組成物、光学部材用粘着剤層およびその製造方法、粘着型光学部材、ならびに画像表示装置
JP2003262729A (ja) 粘着型光学フィルムおよび画像表示装置
JP5341146B2 (ja) 粘着剤付き光学フィルムおよび画像表示装置

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): AE AG AL AM AT AU AZ BA BB BG BR BW BY BZ CA CH CN CO CR CU CZ DE DK DM DZ EC EE EG ES FI GB GD GE GH GM HR HU ID IL IN IS KE KG KP KR KZ LC LK LR LS LT LU LV MA MD MG MK MN MW MX MZ NA NI NO NZ OM PG PH PL PT RO RU SC SD SE SG SK SL SY TJ TM TN TR TT TZ UA UG US UZ VC VN YU ZA ZM ZW

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): BW GH GM KE LS MW MZ NA SD SL SZ TZ UG ZM ZW AM AZ BY KG KZ MD RU TJ TM AT BE BG CH CY CZ DE DK EE ES FI FR GB GR HU IE IS IT LT LU MC NL PL PT RO SE SI SK TR BF BJ CF CG CI CM GA GN GQ GW ML MR NE SN TD TG

121 Ep: the epo has been informed by wipo that ep was designated in this application
DPEN Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed from 20040101)
NENP Non-entry into the national phase

Ref country code: DE

WWW Wipo information: withdrawn in national office

Country of ref document: DE

122 Ep: pct application non-entry in european phase