WO1996034896A1 - A process for hydrogenating aromatic polymers - Google Patents
A process for hydrogenating aromatic polymers Download PDFInfo
- Publication number
- WO1996034896A1 WO1996034896A1 PCT/US1996/005240 US9605240W WO9634896A1 WO 1996034896 A1 WO1996034896 A1 WO 1996034896A1 US 9605240 W US9605240 W US 9605240W WO 9634896 A1 WO9634896 A1 WO 9634896A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- catalyst
- hydrogenation
- percent
- aromatic
- hydrogenated
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J21/00—Catalysts comprising the elements, oxides, or hydroxides of magnesium, boron, aluminium, carbon, silicon, titanium, zirconium, or hafnium
- B01J21/06—Silicon, titanium, zirconium or hafnium; Oxides or hydroxides thereof
- B01J21/08—Silica
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
- B01J23/38—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals
- B01J23/40—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals of the platinum group metals
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
- B01J23/38—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals
- B01J23/40—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals of the platinum group metals
- B01J23/42—Platinum
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
- B01J23/38—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals
- B01J23/40—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of noble metals of the platinum group metals
- B01J23/46—Ruthenium, rhodium, osmium or iridium
- B01J23/464—Rhodium
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J35/00—Catalysts, in general, characterised by their form or physical properties
- B01J35/60—Catalysts, in general, characterised by their form or physical properties characterised by their surface properties or porosity
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08F8/00—Chemical modification by after-treatment
- C08F8/04—Reduction, e.g. hydrogenation
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
- B01J23/70—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper
- B01J23/74—Iron group metals
- B01J23/75—Cobalt
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
- B01J23/70—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper
- B01J23/74—Iron group metals
- B01J23/755—Nickel
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J35/00—Catalysts, in general, characterised by their form or physical properties
- B01J35/60—Catalysts, in general, characterised by their form or physical properties characterised by their surface properties or porosity
- B01J35/61—Surface area
- B01J35/613—10-100 m2/g
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- B01J35/00—Catalysts, in general, characterised by their form or physical properties
- B01J35/60—Catalysts, in general, characterised by their form or physical properties characterised by their surface properties or porosity
- B01J35/66—Pore distribution
Definitions
- the present invention is directed to a process for hydrogenating a high molecular weight aromatic polymer.
- Aromatic polymers have been previously hydrogenated using a variety of catalysts and conditions. Historically, typical hydrogenation catalysts have low reactivity, require high catalyst to polymer ratios and hydrogenate low molecular weight (less than 20,000) aromatic polymers. Hydrogenation of high molecular weight (Mw) aromatic polymers have also required high temperature and/or pressure conditions in order to achieve high o hydrogenation levels. However, these conditions may cause polymer degradation.
- Japanese Patent Application 03076706 describes a process for hydrogenating an aromatic polymer using a silica supported metal hydrogenation catalyst.
- These catalysts use a silica support of small pore diameter (200 to 500 angstroms), high surface area (100-500 m 2 /g) and achieve hydrogenation levels of greater than 70 percent.
- large amounts of catalyst (1-100 weight percent based on resin) and high temperatures (170°C) are required which cause polymer degradation as exemplified by the decrease in the Mw after hydrogenation.
- U.S. Patent No. 5,028,665 describes a process for hydrogenating an unsaturated polymer using a supported metal hydrogenation catalyst wherein the support contains a 0 majority of pores having diameters greater than 450 angstroms.
- the catalyst is limited by a small surface area and enables 90 to 100 percent olefinic hydrogenation but less than 25 percent aromatic hydrogenation.
- U.S. Patent No. 5,352,744 issued to Bates et al. describes a process for hydrogenating poly(alkenyl aromatic) or poly(alkenyl aromatic./polydiene block copolymers, 5 that provides hydrogenated polymers with 99.5 percent or greater saturation, using a metal catalyst on an alkaline metal salt support.
- Bates teaches from 0.01 to 10 grams of catalyst per gram of polymer may be used, a ratio of greater than 1.0 gram of catalyst per gram of polymer is needed to reach high hydrogenation levels.
- Silica has long been used as a support for metal catalysts. Typically, the silica used 0 as a support has had high surface area (200-600 m 2 /g) and small average pore diameter (20 to 40 angstroms). Very low hydrogenation levels are obtained when hydrogenating high molecular weight aromatic polymers using metal hydrogenation catalysts supported by this type of silica.
- the present invention is a process for hydrogenating an aromatic polymer comprising contacting the aromatic polymer with a hydrogenating agent in the presence of a silica supported metal hydrogenation catalyst, characterized in that the silica has a surface area of at least 10 m /g and a pore size distribution such that at least 98 percent of the pore vol ume is defined by pores having diameter of greater than 600 angstroms, and at least 80 percent aromatic hydrogenation is achieved.
- a second aspect of the present invention is a silica supported metal catalyst 5 characterized in that the silica has a surface area of at least 10 m 2 /g and a pore size distribution such that at least 98 percent of the pore volume is defined by pores having diameter of greater than 600 angstroms.
- a third aspect of the present invention is the hydrogenated polymers produced by the process previously described. 1 o Because of the high efficiency of the present catalysts, this process can be used in hydrogenating polystyrene to produce polyvinylcyclohexane without the disadvantages of the prior art.
- the aromatic polymers useful in the process of the present invention include any polymeric material containing pendant aromatic functionality.
- the Mw is from 15 100,000 to 3,000,000, more preferably from 100,000 to 1 ,000,000, and most preferably from
- aromatic polymers 100,000 to 500,000. Although high molecular weight aromatic polymers are preferred, aromatic polymers below 100,000 molecular weight may also be hydrogenated by the process of the present invention.
- Pendant aromatic refers to a structure wherein the aromatic group is a substituent on the polymer backbone and not embedded therein.
- Preferred aromatic groups 0 are C ⁇ - 2 0 aryl groups, especially phenyl. These polymers may also contain other olefinic groups in addition to aromatic groups.
- the polymer is derived from a monomer of the formula:
- R is hydrogen or alkyl
- Ar is phenyl, halophenyl, alkylphenyl, alkylhalophenyl, naphthyl, pyridinyl, or anthracenyl, wherein any alkyl group contains 1 to 6 carbon atoms which may be mono- or multisubstituted with functional groups such as halo, nitro, amino, 0 cyano, carbonyl and carboxyl. More preferablyAr is phenyl or alkylphenyl with phenyl being most preferred. Homopolymers may have any stereostructure including syndiotactic, isotactic or atactic; however, atactic polymers are preferred.
- copolymers containing these aromatic monomers including random, pseudo random, block and grafted copolymers may be used.
- copolymers of vinyl aromatic monomers and comonomers selected from 5 nitriles, acrylates, acids, ethylene, propylene, maleic anhydride, maleimides, vinyl acetate, and vinyl chloride may also be used such as styrene-acrylonitrile, styrene-alpha-methylstyrene and styrene-ethylene.
- Block copolymers of vinyl aromatic monomers and conjugated dienes such as butadiene, isoprene may also be used.
- Examples include styrene-butadiene, styrene-isoprene, styrene-butadiene-styrene and styrene-isoprene-styrene copolymers. Further examples of block copolymers may be found in U.S. Patents 4,845, 173, 4,096,203, 4,200,718, 4,201 ,729, 4,205,016, 3,652,516, 3,734,973, 3,390,207, 3,231,635, and 3,030,346. Blends of polymers including impact modified, grafted rubber containing aromatic polymers may also be used.
- the silica support used in the process of the present invention has a narrow pore size distribution and surface area greaterthan 10 meters squared per gram (m 2 /g).
- the pore size distribution, pore volume, and average pore diameter can be obtained via mercury porosimetry following the proceedings of ASTM D-4284-83.
- the pore size distribution is typically measured using mercury porosimetry. However, this method is only sufficient for measuring pores of greater than 60 angstroms. Therefore, an additional method must be used to measure pores less than 60 angstroms.
- One such method is nitrogen desorption according to ASTM D-4641-87 for pore diameters of less than 600 angstroms. Therefore, narrow pore size distribution is defined as the requirement that at least 98 percent of the pore volume is defined by pores having pore diameters greater than 600 angstroms and that the pore volume measured by nitrogen desorption for pores less than 600 angstroms, be less than 2 percent of the total pore volume measured by mercury porosimetry.
- the surface area can be measured according to ASTM D-3663-84.
- the surface area is typically between 10 and 50 m 2 /g, preferably between 12 and 20 with most preferred between 14 and 17 m 2 /g.
- the desired average pore diameter is dependent upon the aromatic polymer which is to be hydrogenated and its molecular weight. It is preferable to use supports having higher average pore diameters for the hydrogenation of polymers having higher molecular weights to obtain the desired amount of hydrogenation.
- Average pore diameters are typically between 1000 and 5000 angstroms, preferably between 3000 and 4000 angstroms, most preferably between 3500 and 4000 angstroms. Pore diameters of greater than 5000 angstroms may also be used if the surface area is maintained at the levels specified.
- the si I ica used as the support i n the process of the present i nvention can be made by combining potassium silicate in water with a gelation agent, such as formamide, polymerizing and leaching as exemplified in U.S. Patent No. 4,1 12,032.
- the silica is then hydrothermally calcined as in Her, R.K., The Chemistry of Silica, John Wiley and Sons, 1979, pp. 539-544, which generally consists of heating the silica while passing a gas saturated with water over the silica fo 2 hours or more at temperatures from 600°Cto 850°C. Hydrothermal calcining results in a narrowing of the pore diameter distribution as well as increasing the average pore diameter.
- the metal used in the hydrogenation catalyst can be any metal which will increase the rate of hydrogenation including nickel, cobalt, rhodium, ruthenium, palladium, platinum, other Group VIM metals, or combinations thereof.
- rhodium or platinum is used.
- platinum is known to be a poor hydrogenation catalyst for nitriles, therefore, platinum would not be preferred in the hydrogenation of nitrile copolymers.
- the silica supported catalyst can be made using the supports described herein, by the process described in U.S. Patent No. 5,110,779.
- An appropriate metal or metal containing compound can be deposited on the support by vapor phase deposition, aqueous or nonaqueous impregnation followed by calcination, sublimation or any other conventional method, such as those exemplified in Studies in Surface Science and Catalysis, "Successful Design of Catalysts" V.44, pg. 146-158, 1989 and Applied Heterogeneous Catalysis pqs. 75-123, Institute Fran ⁇ ais du P ⁇ trole Publications, 1987.
- the appropriate metal containing compound can be any compound containing a metal, as previously described, which will produce a usable hydrogenation catalyst.
- These compounds can be salts, coordination complexes, organometallic compounds or covending complexes and are preferably metal halide salts with metal chloride salts being most preferred.
- the metal is 0.1 to 10 wt. percent of the silica supported catalyst. Preferable amounts are from 0.5 to 8 wt. percent, more preferably 1 to 5 wt. percent based on total catalyst weight.
- Promoters such as alkali, alkali earth or lanthanide containing compounds, can also be used to aid in the dispersion of the metal onto the silica support or stabilization during the reaction, though their use is not preferred.
- the amount of catalyst used in the hydrogenation process is much smallerthan the amount required in conventional aromatic polymer hydrogenation reactions due to the high reactivity of the present catalysts. Generally, amounts of less than 1 gram of catalyst per gram of aromatic polymer are used, with less than 0.1 gram being preferred and less than 0.05 being more preferred.
- the amount of catalyst used is dependent upon the type of process, whether it is continuous, semi-continuous or batch, and the process conditions, such as temperature, pressure and reaction time wherein typical reaction times may vary from 5 minutes to ⁇ hours.
- Continuous operations can typically contain 1 part by weight catalyst to 200,000 or more parts aromatic polymer since the catalyst is reused many times during the course of continuous operation. Typical batch processes can use 1 part by weight catalyst to 5,000 parts aromatic polymer. Higher temperatures and pressures will also enable using smaller amounts of catalyst.
- the hydrogenation reaction can be conducted in the absence of a solvent but is preferably conducted in a hydrocarbon solvent in which the polymer is soluble and which will not hinder the hydrogenation reaction.
- the solvent is a saturated solvent such as cyclohexane, methylcyclohexane, ethylcyclohexane, cyclooctane, cycloheptane, dodecane, dioxane, diethylene glycol dimethyl ether, tetrahydrofuran, isopentane, decahydronaphthalene or mixtures thereof, with cyclohexane being the most preferred.
- the temperature at which the hydrogenation is conducted can be any temperature at which hydrogenation occurs without significant degradation of the polymer.
- Degradation of the polymer can be detected by a decrease in Mw, an increase in polydispersity or a decrease in glass transition temperature, after hydrogenation.
- Significant degradation in polymers having a polydispersity between 1.0 and 1.2 can be defined as an increase of 30 percent or more in polydispersity after hydrogenation.
- polymer degradation is such that less than a 20 percent increase in polydispersity occurs after hydrogenation, most preferably less than 10 percent.
- a significant decrease in molecular weight after hydrogenation indicates that degradation has occurred.
- Significant degradation in this case is defined as a decrease in Mw of 20 percent or more.
- a Mw decrease after hydrogenation will be less than 10 percent.
- o polymers such as poly-alpha-methylstyrene or other alpha substituted vinyl aromatic polymers which are more prone to polymer degradation, can tolerate a decrease in Mw of up to 30 percent.
- Typical hydrogenation temperatures are from 50°C preferably from 100°C, more preferably from 110°C, and most preferably from 120°Cto 250°C, preferably to 200°C, more 5 preferably to 180°C, and most preferably to 160°C.
- the pressure of the hydrogenation reaction is not critical, though hydrogenation rates increase with increasing pressure. Typical pressures range from atmospheric pressure to 10,000 psig with 500 to 1500 psig being preferred.
- the reaction vessel is purged with an inert gas to remove oxygen from the 0 reaction area.
- Inert gases include but are not limited to nitrogen, helium, and argon, with nitrogen being preferred.
- the hydrogenating agent can be any hydrogen producing agent which will efficiently hydrogenatethe aromatic polymer.
- Hydrogenating agents include but are not limited to hydrogen gas, hydrazine and sodium borohydride.
- the 5 hydrogenating agent is hydrogen gas.
- the amount of hydrogenation can be measured using UV-VIS spectroscopy. Cyclohexane solutions of polystyrene give a very distinct absorption band for the aromatic ring at 260.5 nm. This band gives an absorbance of 1.000 with a solution concentration of .004980 moles of aromatic per liter in a 1 cm cell. After removing the catalyst via filtration (using a 0.50 0 micrometer (lm) "TEFLONTM " filter, Millipore FHUP047) the reaction mixture is placed in a UV cell and the absorbance measured. The absorbance is dependent upon concentration. The hydrogenated polymer products are typically measured at higher concentrations since they are not diluted before the absorbance is measured. Since the reaction solution is 15-30 times more concentrated than the standards, small amounts of residual unsaturation can be accurately 5 measured.
- the amount of hydrogenation is dependent upon the polymer being hydrogenated, the amount of catalyst used, the process conditions and the reaction time.
- a typical hydrogenation is greater than 80 percent, greater than 99 percent hydrogenation is preferred, more preferably greater than 99.5 percent, and most preferably greater than 99.9 percent. This can be determined by measuring the absorbance of the hydrogenated polymer and comparing to the absorbance of a nonhydrogenated standard. In other words, the absorbance of a 99.9 percent hydrogenated polymer will be 99.9 percent less than the absorbance of the nonhydrogenated polymer.
- the level of hydrogenation can be lower, and is dependent upon the polymer being hydrogenated.
- at least 10 percent hydrogenation is achieved, preferably at least 25 percent, more preferably at least 50 percent and most preferably at least 90 percent hydrogenation is achieved.
- the aromatic polymer is typically dissolved in a solvent and placed in a reactor with an appropriate amount of silica supported hydrogenation catalyst.
- the reactor is sealed, purged with an inert gas, pressurized with hydrogen and heated to the desired temperature for a time sufficient to substantially hydrogenate the aromatic polymer.
- the hydrogenated polymer is removed and the catalyst can be separated from the hydrogenated polymer by any conventional catalyst separation method, such as filtration or centrifugation.
- T e hydrogenated polymers of the present invention have higher glass transition temperatures than their nonhydrogenated counterparts.
- atactic hydrogenated polystyrene polymers of the present invention typically have glass transition temperatures measured by Differential Scanning Calorimetry (DSC) with a heating rate of 3°C per minute, of at least 141°C, preferably from 141°Cto 147°C, more preferably from 143°Cto 147°C, and most preferably from 145°C to 147°C. Therefore, these polymers can be used in applications where high temperature resistance is required, such as applications where polycarbonates currently are used.
- DSC Differential Scanning Calorimetry
- the amount of hydrogenation is measured using UV-VIS spectroscopy as described previously.
- Mw is an absolute molecular weight measured by gel permeation chromatography, unless otherwise specified. All polymer samples used in the examples have atactic stereostructure.
- potassium silicate (Kasil #1 , a product of PQ Corp.) and 10 g of water is
- Table I Three additional batches are prepared using the same procedure described above and are 5 shown in Table I.
- the surface area of Table I is measured according to ASTM method D-3663-84.
- the silica as prepared in Sample 1 above has a cumulative pore volume in pores of less than 100 angstroms of 0.006 cc/g, a cumulative pore volume in pores of less than 320 angstroms of 0.013 cc/g and a cumulative pore volume in pores of less than 600 angstroms of 0.016 cc/g. Therefore, the cumulative pore volume for pores less than 600 angstroms is 1.1 percent of the cumulative pore volume for pores greater than 60 angstroms.
- Rh/Si0 2 catalyst is made via impregnation of the hydrothermally 5 calcined silica of (A).
- RhCI 3 (H 2 0) 2 5 (0.65 g) is dissolved in 16.5 ml of water. This solution is then added to 5.0 g of the hydrothermally calcined silica of (A), which is then air dried overnight.
- the catalyst is then ground with a mortar and pestle to less than 100 mesh.
- the catalyst is reduced by loading the catalyst in a 1.0 in. O.D. glass tube purged with nitrogen and then a flow of hydrogen is started over the catalyst.
- the temperature is ramped from 25°Cto 250°C at 10 10°C/min in flowing hydrogen and the catalyst is held isothermally at 250°C for 2 hours.
- the catalyst is cooled under flowing hydrogen.
- a 5 percent Pt Si0 2 catalyst is made via impregnation of the hydrothermally calcined silica of (A).
- H 2 PtCI 6 .6(H 2 0) (0.70 g) is dissolved in 16.5 ml of water. This solution is 15 then added to 5.0 g of the hydrothermally calcined silica of (A) which is then air dried overnight.
- the catalyst is then ground with a mortar and pestle to less than 100 mesh.
- the catalyst is reduced by loading the catalyst in a 1.0 in. O.D. glass tube purged with nitrogen and then a flow of hydrogen is started over the catalyst. The temperature is ramped from 25°Cto
- the reactors are sealed, pressure purged with nitrogen and finally pressurized with hydrogen to 1300 psig.
- the reactors are then heated to 130°C, the pressure adjusted to 1500 psig and the reaction run for 4 hours.
- the results are listed in Table II.
- Pd/BaSO 4 The level of hydrogenation for the catalyst of the invention is measured at greater than 99.9 percent at a catalyst to polymer ratio of 0.27 and Mw/Mn is measured to be 1.10, which indicates that no significant polymer degradation has occurred.
- Four analyses of the hydrogenated polymer give an average Tg of 146.2°C ⁇ 0.5.
- a Pd metal catalyst supported on an alkaline earth metal support used at a catalyst to polymer ratio of 0.3 shows very low hydrogenation.
- Example 3 The silica supported catalysts were prepared as in Example 1, (B1) and (B2). The reactor is sealed and pressure purged with nitrogen and finally pressurized with hydrogen to
- the catalysts of the present invention give much higher hydrogenation levels at a catalyst to polymer ratio of 0.27 than a known hydrogenation catalyst.
- Four analyses of the 2 5 hydrogenated polymer using 5 percent Pt/Si0 catalyst give an average Tg of 146.6°C ⁇ 0.6.
- polystyrene (Mw approximately 200,000) is added to a 5 gallon reactor containing 2300 g of cyclohexane.
- the reactor is purged with nitrogen and 13.5 g of a reduced 5 percent Pt/Si0 2 catalyst prepared as in Example 1 , (B2) is added.
- the reactor is sealed, pressure purged with nitrogen, pressurized with hydrogen to 500 psig and heated to 150°C.
- the pressure is adjusted to 875 psig and maintained at this pressure at 150°C. Samples taken after 55 minutes show hydrogenation of 94.3 percent and samples taken after 110 minutes show hydrogenation of 98.4 percent.
- LALLS Laser Light Scattering
Landscapes
- Chemical & Material Sciences (AREA)
- Organic Chemistry (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Health & Medical Sciences (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- General Chemical & Material Sciences (AREA)
- Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
- Catalysts (AREA)
- Silicon Compounds (AREA)
- Organic Low-Molecular-Weight Compounds And Preparation Thereof (AREA)
Priority Applications (7)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| BR9608697A BR9608697A (pt) | 1995-05-04 | 1996-04-16 | Processo para hidrogenar um polímero aromático catalisador metálico suportado por silica polímero hidrogenado copolímero hidrogenado e homopolímero hidrogenado |
| DE69602743T DE69602743T2 (de) | 1995-05-04 | 1996-04-16 | Verfahren zur hydrogenierung von aromatischen polymeren |
| MX9708469A MX9708469A (es) | 1995-05-04 | 1996-04-16 | Un proceso para hidrogenar polimeros aromaticos. |
| EP96912797A EP0823916B1 (en) | 1995-05-04 | 1996-04-16 | A process for hydrogenating aromatic polymers |
| HK98109131.4A HK1008229B (en) | 1995-05-04 | 1996-04-16 | A process for hydrogenating aromatic polymers |
| JP53332796A JP4111540B2 (ja) | 1995-05-04 | 1996-04-16 | 芳香族ポリマーの水素化法 |
| AU55487/96A AU703098B2 (en) | 1995-05-04 | 1996-04-16 | A process for hydrogenating aromatic polymers |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US08/434,636 | 1995-05-04 | ||
| US08/434,636 US5612422A (en) | 1995-05-04 | 1995-05-04 | Process for hydrogenating aromatic polymers |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1996034896A1 true WO1996034896A1 (en) | 1996-11-07 |
Family
ID=23725021
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1996/005240 Ceased WO1996034896A1 (en) | 1995-05-04 | 1996-04-16 | A process for hydrogenating aromatic polymers |
Country Status (13)
| Country | Link |
|---|---|
| US (3) | US5612422A (enExample) |
| EP (2) | EP0823916B1 (enExample) |
| JP (1) | JP4111540B2 (enExample) |
| CN (2) | CN1117103C (enExample) |
| AU (1) | AU703098B2 (enExample) |
| BR (1) | BR9608697A (enExample) |
| CA (1) | CA2217207A1 (enExample) |
| CO (1) | CO4560454A1 (enExample) |
| DE (2) | DE69628304T2 (enExample) |
| ES (1) | ES2132918T3 (enExample) |
| MX (1) | MX9708469A (enExample) |
| TW (1) | TW419488B (enExample) |
| WO (1) | WO1996034896A1 (enExample) |
Cited By (21)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1999032526A3 (de) * | 1997-12-18 | 1999-12-23 | Bayer Ag | Verfahren zur hydrierung aromatischer polymere |
| WO2000005278A1 (de) * | 1998-07-23 | 2000-02-03 | Bayer Aktiengesellschaft | Verfahren zur hydrierung aromatischer polymere in gegenwart von sauerstoffenthaltenden kohlenwasserstoffen |
| WO2000005279A1 (de) * | 1998-07-23 | 2000-02-03 | Bayer Aktiengesellschaft | Verfahren zur hydrierung aromatischer polymere in gegenwart spezieller katalysatoren |
| WO2000077094A1 (en) * | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| WO2000077095A1 (en) * | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| WO2001009239A1 (en) * | 1999-07-28 | 2001-02-08 | The Dow Chemical Company | Hydrogenated block polymers having elasticity and articles made therefrom |
| WO2001023437A1 (en) * | 1999-09-28 | 2001-04-05 | Teijin Limited | Optical material comprising star-shaped hydrogenated polystyrene block copolymer, process for producing the same, and substrate for optical disk |
| WO2001042319A1 (en) * | 1999-12-08 | 2001-06-14 | The Dow Global Technologies Inc. | A process for hydrogenating unsaturated polymers |
| WO2001042355A1 (en) * | 1999-12-07 | 2001-06-14 | Dow Global Technologies Inc. | Hydrogenated block copolymer compositions for thin wall injection molding applications |
| WO2001074912A1 (en) * | 2000-04-03 | 2001-10-11 | Dow Global Technologies Inc. | A process for preparing hydrogenated aromatic polymers |
| US6365694B1 (en) | 1997-12-18 | 2002-04-02 | Bayer Aktiengesellschaft | Amorphous vinyl cyclohexane polymers |
| US6426390B1 (en) | 1999-06-11 | 2002-07-30 | Dow Global Technology Inc. | Hydrogenated block copolymer compositions |
| EP1277768A1 (en) * | 2001-07-18 | 2003-01-22 | ATOFINA Research | Polymer hydrogenation process |
| US6632890B1 (en) | 1999-03-19 | 2003-10-14 | Dow Global Technologies Inc. | Hydrogenated block copolymer compositions |
| US6777082B2 (en) | 1999-07-28 | 2004-08-17 | The Dow Chemical Company | Hydrogenated block copolymers having elasticity and articles made therefrom |
| US6815475B2 (en) | 1999-06-11 | 2004-11-09 | Dow Global Technologies Inc. | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| US6914091B2 (en) | 1999-06-11 | 2005-07-05 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| US6916879B2 (en) | 2001-05-18 | 2005-07-12 | Basf Aktiengesellschaft | Core-hydrogenated block copolymers having an asymmetric structure |
| US7355084B2 (en) | 2001-06-11 | 2008-04-08 | Basf Aktiengesellschaft | Method for hydrogenating organic compounds by means of Ru/SiO2 catalysts |
| CN102219223A (zh) * | 2011-03-14 | 2011-10-19 | 杭州华品科技有限公司 | 一种超宽孔二氧化硅载体的制备方法 |
| US10553818B2 (en) | 2016-03-18 | 2020-02-04 | Zeon Corporation | Method for manufacturing organic electronic device sealing body |
Families Citing this family (48)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP0989417A4 (en) * | 1997-06-06 | 2001-10-17 | Nippon Zeon Co | SHAPED MATERIAL FOR PLASTIC LENSES |
| US6172165B1 (en) * | 1997-07-24 | 2001-01-09 | The Dow Chemical Company | Process for hydrogenating aromatic polymers |
| DE19815737A1 (de) * | 1998-04-08 | 1999-10-14 | Bayer Ag | Verfahren zur Hydrierung aromatischer Polymere in Gegenwart verzweigter Kohlenwasserstoffe |
| US6030680A (en) * | 1998-09-04 | 2000-02-29 | The Dow Chemical Company | Adhesion of amorphous saturated hydrocarbon thermoplastic substrates |
| DE19855062A1 (de) | 1998-11-28 | 2000-05-31 | Bayer Ag | Blockcopolymere auf Vinylcyclohexanbasis |
| EP1193274B1 (en) * | 1998-12-04 | 2006-05-31 | Nippon Zeon Co., Ltd. | Resin composition comprising hydrogenated polymers and process for producing substrate for information-recording medium |
| DE19904612A1 (de) | 1999-02-05 | 2000-08-10 | Bayer Ag | Verfahren zur Hydrierung aromatischer Polymere in Gegenwart spezieller Katalysatoren |
| WO2000077054A1 (en) | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Hydrogenated block copolymers and optical media discs produced therefrom |
| WO2000077053A1 (en) | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Hydrogenated block copolymers and optical media discs produced therefrom |
| US6376622B1 (en) * | 1999-12-08 | 2002-04-23 | The Dow Chemical Company | Process for hydrogenating aromatic polymers |
| US20030099837A1 (en) * | 1999-12-22 | 2003-05-29 | Dirk Mockel | Thermoplastic multi-layered film with a layer of vinylcyclohexane-based polymer |
| US20030139535A1 (en) * | 2000-03-01 | 2003-07-24 | Hironori Haga | Process for producing hydrogenated unsaturated ring-containing hydrocarbon polymer |
| WO2001070833A1 (en) * | 2000-03-23 | 2001-09-27 | Dow Global Technologies Inc. | Hydrogenated monovinylidene aromatic polymer compositions |
| US6455656B2 (en) | 2000-04-03 | 2002-09-24 | Dow Global Technologies Inc. | Process for preparing hydrogenated aromatic polymers |
| US6395841B1 (en) * | 2000-09-06 | 2002-05-28 | The Dow Chemical Company | Process for hydrogenating unsaturated polymers |
| AU2003218113A1 (en) * | 2002-03-11 | 2003-09-29 | Dow Global Technologies Inc. | Stretch fabric with improved chemical resistance and durability |
| JP3996008B2 (ja) * | 2002-07-31 | 2007-10-24 | 株式会社ブリヂストン | ゴム組成物及びこれをトレッドに用いた空気入りタイヤ |
| WO2004052937A2 (en) * | 2002-11-05 | 2004-06-24 | North Carolina State University | Hydrogenation of polymers in the presence of supercritical carbon dioxide |
| US7053156B2 (en) * | 2003-12-19 | 2006-05-30 | Kraton Polymers U.S. Llc | Process for hydrogenating block copolymers |
| CN102229816A (zh) | 2005-01-14 | 2011-11-02 | 埃克森美孚化学专利公司 | 超纯流体 |
| JPWO2006101079A1 (ja) * | 2005-03-24 | 2008-09-04 | 出光興産株式会社 | 脱硫剤及びこれを用いた脱硫方法 |
| TWI396701B (zh) * | 2006-02-27 | 2013-05-21 | Mitsubishi Gas Chemical Co | 氫化聚合物之製法 |
| WO2008045181A1 (en) | 2006-10-05 | 2008-04-17 | Dow Global Technologies Inc. | Bulk light diffuser composition |
| JP5540703B2 (ja) | 2007-08-06 | 2014-07-02 | 三菱瓦斯化学株式会社 | 核水素化された芳香族ビニル化合物/(メタ)アクリレート系共重合体の製造方法 |
| WO2009050292A2 (en) | 2007-10-19 | 2009-04-23 | Shell Internationale Research Maatschappij B.V. | Catalyst for the hydrogenation of unsaturated hydrocarbons and process for its preparation |
| EP2212728A1 (en) * | 2007-11-20 | 2010-08-04 | Dow Global Technologies Inc. | Optical compensation film |
| TWI388577B (zh) | 2008-12-30 | 2013-03-11 | Tsrc Corp | 製造高度氫化的嵌段共聚物之方法 |
| WO2011061575A1 (en) * | 2009-11-20 | 2011-05-26 | Total Raffinage Marketing | Process for the production of hydrocarbon fluids having a low aromatic content |
| WO2011061576A1 (en) | 2009-11-20 | 2011-05-26 | Total Raffinage Marketing | Process for the production of hydrocarbon fluids having a low aromatic content |
| JP5841949B2 (ja) | 2009-12-18 | 2016-01-13 | ダウ グローバル テクノロジーズ エルエルシー | 環状ブロックコポリマーを含むプラスチック光ファイバ |
| CN103347903B (zh) | 2010-07-28 | 2016-03-16 | 朗盛德国有限责任公司 | 基于二烯的聚合物的氢化 |
| CN102513080B (zh) * | 2011-11-23 | 2014-01-15 | 华东理工大学 | 环己烷基乙烯的均聚物或共聚物的制备方法及一种催化剂 |
| TWI494335B (zh) | 2012-08-31 | 2015-08-01 | 台橡股份有限公司 | 氫化聚合物的方法及其氫化聚合物 |
| ES2613859T3 (es) * | 2012-10-08 | 2017-05-26 | Shell Internationale Research Maatschappij B.V. | Proceso para la licuación de un material celulósico |
| CN104140480B (zh) * | 2013-05-08 | 2016-10-19 | 中国石油大学(北京) | 一种聚苯乙烯加氢制备聚环己基乙烯的方法 |
| TWI558727B (zh) | 2013-09-30 | 2016-11-21 | 陶氏全球科技有限責任公司 | 製備聚烯烴反應性遙爪預聚合物之方法、聚烯烴反應性遙爪預聚合物及交聯彈性體以及高分子量彈性體 |
| FR3015514B1 (fr) | 2013-12-23 | 2016-10-28 | Total Marketing Services | Procede ameliore de desaromatisation de coupes petrolieres |
| SG11201605672PA (en) | 2014-01-14 | 2016-08-30 | Dow Global Technologies Llc | A process to produce polyolefin ionomers and ionomers produced thereby |
| WO2016130639A1 (en) * | 2015-02-11 | 2016-08-18 | Polyone Corporation | Super-vibration damping thermoplastic elastomer blends |
| US11298922B2 (en) | 2016-02-24 | 2022-04-12 | BMSI, Inc. | Packaging laminate |
| US11235561B2 (en) | 2016-02-24 | 2022-02-01 | BMSI, Inc. | Packaging laminate |
| EP3452263B1 (en) | 2016-03-11 | 2022-10-19 | Polyplastics Usa, Inc. | Injection stretch blow-molding (isbm) enhancement for semi-crystalline polyolefin containers utilizing alicyclic polyolefins |
| US10814593B2 (en) | 2016-07-25 | 2020-10-27 | Avient Corporation | Super-vibration damping thermoplastic elastomer blends and articles made therewith |
| JP6749502B2 (ja) | 2017-02-17 | 2020-09-02 | スリーエム イノベイティブ プロパティズ カンパニー | トリブロックコポリマー |
| WO2019118331A1 (en) * | 2017-12-11 | 2019-06-20 | Valvoline Licensing And Intellectual Property Llc | Scalable synthesis of hydrogenated alpha styrene dimer |
| WO2019229680A1 (en) | 2018-06-01 | 2019-12-05 | 3M Innovative Properties Company | Porous membranes including triblock copolymers |
| CN116018206A (zh) * | 2020-07-14 | 2023-04-25 | 沙特基础工业全球技术公司 | 用于氢化含芳香环的聚合物的催化剂及其用途 |
| AU2022275829B2 (en) | 2021-05-19 | 2026-02-12 | China Petroleum & Chemical Corporation | Hydrogenation method for aromatic polymer and hydrogenated block copolymer and use thereof |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE2845615A1 (de) * | 1977-10-20 | 1979-04-26 | Johnson Matthey Co Ltd | Stabilisierter polymer und verfahren zum hydrieren von polymeren, copolymeren sowie fuer das selektive hydrieren von block-copolymeren |
| DE3227650A1 (de) * | 1981-07-24 | 1983-03-17 | Nippon Zeon Co., Ltd., Tokyo | Verfahren zur hydrierung von konjugierten dienpolymeren |
| US4629767A (en) * | 1985-07-12 | 1986-12-16 | Phillips Petroleum Co. | Hydrogenation process and catalyst |
| EP0378104A2 (en) * | 1989-01-09 | 1990-07-18 | The Dow Chemical Company | Polymer hydrogenation catalysts |
| JPH0376706A (ja) * | 1989-08-21 | 1991-04-02 | Mitsubishi Kasei Corp | 水素化スチレン系樹脂の製造方法 |
Family Cites Families (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US3888972A (en) * | 1972-05-11 | 1975-06-10 | Andrei Vladimirovich Kiselev | Process for preparation of wide-pore adsorbent for use in chromatography |
| US4112032A (en) * | 1976-04-21 | 1978-09-05 | Corning Glass Works | Silica-containing porous bodies of controlled pore size |
| US4617060A (en) * | 1984-04-23 | 1986-10-14 | Mallinckrodt, Inc. | Silica catalyst supports |
| US4976848A (en) * | 1988-10-04 | 1990-12-11 | Chevron Research Company | Hydrodemetalation and hydrodesulfurization using a catalyst of specified macroporosity |
| US5110779A (en) * | 1989-01-09 | 1992-05-05 | The Dow Chemical Company | Polymer hydrogenation catalysts |
| JP2890748B2 (ja) * | 1990-08-24 | 1999-05-17 | 三菱化学株式会社 | 水素化スチレン系樹脂の製造方法 |
| JPH04108809A (ja) * | 1990-08-29 | 1992-04-09 | Japan Synthetic Rubber Co Ltd | 重合体の水素化方法 |
| CA2084929C (en) * | 1991-12-30 | 2000-01-25 | Exxon Research And Engineering Company | Catalyst and process for cracking hydrocarbons with highly attrition resistant mesoporous catalytic cracking catalysts |
| US5352744A (en) * | 1993-03-15 | 1994-10-04 | University Of Minnesota | Method for hydrogenating polymers and products therefrom |
-
1995
- 1995-05-04 US US08/434,636 patent/US5612422A/en not_active Expired - Lifetime
-
1996
- 1996-04-03 US US08/627,206 patent/US5654253A/en not_active Expired - Lifetime
- 1996-04-03 US US08/627,203 patent/US5700878A/en not_active Expired - Lifetime
- 1996-04-16 WO PCT/US1996/005240 patent/WO1996034896A1/en not_active Ceased
- 1996-04-16 EP EP96912797A patent/EP0823916B1/en not_active Expired - Lifetime
- 1996-04-16 CN CN96193724.6A patent/CN1117103C/zh not_active Expired - Lifetime
- 1996-04-16 JP JP53332796A patent/JP4111540B2/ja not_active Expired - Lifetime
- 1996-04-16 CN CNB00131663XA patent/CN1177866C/zh not_active Expired - Lifetime
- 1996-04-16 ES ES96912797T patent/ES2132918T3/es not_active Expired - Lifetime
- 1996-04-16 DE DE69628304T patent/DE69628304T2/de not_active Expired - Lifetime
- 1996-04-16 EP EP98103008A patent/EP0842698B1/en not_active Expired - Lifetime
- 1996-04-16 CA CA002217207A patent/CA2217207A1/en not_active Abandoned
- 1996-04-16 AU AU55487/96A patent/AU703098B2/en not_active Ceased
- 1996-04-16 BR BR9608697A patent/BR9608697A/pt not_active Application Discontinuation
- 1996-04-16 MX MX9708469A patent/MX9708469A/es not_active IP Right Cessation
- 1996-04-16 DE DE69602743T patent/DE69602743T2/de not_active Expired - Lifetime
- 1996-04-30 CO CO96021443A patent/CO4560454A1/es unknown
- 1996-05-03 TW TW085105318A patent/TW419488B/zh not_active IP Right Cessation
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE2845615A1 (de) * | 1977-10-20 | 1979-04-26 | Johnson Matthey Co Ltd | Stabilisierter polymer und verfahren zum hydrieren von polymeren, copolymeren sowie fuer das selektive hydrieren von block-copolymeren |
| DE3227650A1 (de) * | 1981-07-24 | 1983-03-17 | Nippon Zeon Co., Ltd., Tokyo | Verfahren zur hydrierung von konjugierten dienpolymeren |
| US4629767A (en) * | 1985-07-12 | 1986-12-16 | Phillips Petroleum Co. | Hydrogenation process and catalyst |
| EP0378104A2 (en) * | 1989-01-09 | 1990-07-18 | The Dow Chemical Company | Polymer hydrogenation catalysts |
| JPH0376706A (ja) * | 1989-08-21 | 1991-04-02 | Mitsubishi Kasei Corp | 水素化スチレン系樹脂の製造方法 |
Non-Patent Citations (1)
| Title |
|---|
| CHEMICAL ABSTRACTS, vol. 115, no. 8, 26 August 1991, Columbus, Ohio, US; abstract no. 72525r, "MANUFACTURE OF HYDROGENATED POLYSTYRENE RESINS" page 22; XP002007781 * |
Cited By (27)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6365694B1 (en) | 1997-12-18 | 2002-04-02 | Bayer Aktiengesellschaft | Amorphous vinyl cyclohexane polymers |
| WO1999032526A3 (de) * | 1997-12-18 | 1999-12-23 | Bayer Ag | Verfahren zur hydrierung aromatischer polymere |
| US6417287B1 (en) | 1997-12-18 | 2002-07-09 | Bayer Aktiengesellschaft | Method for hydrogenating aromatic polymers |
| AU760564B2 (en) * | 1998-07-23 | 2003-05-15 | Bayer Aktiengesellschaft | Method for hydrogenating aromatic polymers in the presence of special catalysts |
| WO2000005279A1 (de) * | 1998-07-23 | 2000-02-03 | Bayer Aktiengesellschaft | Verfahren zur hydrierung aromatischer polymere in gegenwart spezieller katalysatoren |
| WO2000005278A1 (de) * | 1998-07-23 | 2000-02-03 | Bayer Aktiengesellschaft | Verfahren zur hydrierung aromatischer polymere in gegenwart von sauerstoffenthaltenden kohlenwasserstoffen |
| US6509510B1 (en) | 1998-07-23 | 2003-01-21 | Bayer Aktiengesellschaft | Method for hydrogenating aromatic polymers in the presence of special catalysts |
| US6420491B1 (en) | 1998-07-23 | 2002-07-16 | Bayer Aktiengesellschaft | Method for hydrogenating aromatic polymers in the presence of hydrocarbons which contain oxygen |
| US6632890B1 (en) | 1999-03-19 | 2003-10-14 | Dow Global Technologies Inc. | Hydrogenated block copolymer compositions |
| US6426390B1 (en) | 1999-06-11 | 2002-07-30 | Dow Global Technology Inc. | Hydrogenated block copolymer compositions |
| US6914091B2 (en) | 1999-06-11 | 2005-07-05 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| WO2000077094A1 (en) * | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| US6815475B2 (en) | 1999-06-11 | 2004-11-09 | Dow Global Technologies Inc. | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| WO2000077095A1 (en) * | 1999-06-11 | 2000-12-21 | The Dow Chemical Company | Compositions comprising hydrogenated block copolymers and end-use applications thereof |
| WO2001009239A1 (en) * | 1999-07-28 | 2001-02-08 | The Dow Chemical Company | Hydrogenated block polymers having elasticity and articles made therefrom |
| US6777082B2 (en) | 1999-07-28 | 2004-08-17 | The Dow Chemical Company | Hydrogenated block copolymers having elasticity and articles made therefrom |
| WO2001023437A1 (en) * | 1999-09-28 | 2001-04-05 | Teijin Limited | Optical material comprising star-shaped hydrogenated polystyrene block copolymer, process for producing the same, and substrate for optical disk |
| WO2001042355A1 (en) * | 1999-12-07 | 2001-06-14 | Dow Global Technologies Inc. | Hydrogenated block copolymer compositions for thin wall injection molding applications |
| WO2001042319A1 (en) * | 1999-12-08 | 2001-06-14 | The Dow Global Technologies Inc. | A process for hydrogenating unsaturated polymers |
| US6399538B1 (en) | 1999-12-08 | 2002-06-04 | The Dow Chemical Company | Process for hydrogenating unsaturated polymers |
| WO2001074912A1 (en) * | 2000-04-03 | 2001-10-11 | Dow Global Technologies Inc. | A process for preparing hydrogenated aromatic polymers |
| US6916879B2 (en) | 2001-05-18 | 2005-07-12 | Basf Aktiengesellschaft | Core-hydrogenated block copolymers having an asymmetric structure |
| US7355084B2 (en) | 2001-06-11 | 2008-04-08 | Basf Aktiengesellschaft | Method for hydrogenating organic compounds by means of Ru/SiO2 catalysts |
| WO2003008467A1 (en) * | 2001-07-18 | 2003-01-30 | Atofina Research | Polymer hydrogenation process |
| EP1277768A1 (en) * | 2001-07-18 | 2003-01-22 | ATOFINA Research | Polymer hydrogenation process |
| CN102219223A (zh) * | 2011-03-14 | 2011-10-19 | 杭州华品科技有限公司 | 一种超宽孔二氧化硅载体的制备方法 |
| US10553818B2 (en) | 2016-03-18 | 2020-02-04 | Zeon Corporation | Method for manufacturing organic electronic device sealing body |
Also Published As
| Publication number | Publication date |
|---|---|
| DE69602743T2 (de) | 1999-10-07 |
| JP4111540B2 (ja) | 2008-07-02 |
| DE69628304D1 (de) | 2003-06-26 |
| DE69628304T2 (de) | 2004-04-01 |
| MX9708469A (es) | 1998-02-28 |
| TW419488B (en) | 2001-01-21 |
| CN1177866C (zh) | 2004-12-01 |
| JPH11504959A (ja) | 1999-05-11 |
| DE69602743D1 (de) | 1999-07-08 |
| EP0842698B1 (en) | 2003-05-21 |
| ES2132918T3 (es) | 1999-08-16 |
| US5612422A (en) | 1997-03-18 |
| US5700878A (en) | 1997-12-23 |
| EP0842698A2 (en) | 1998-05-20 |
| CN1403490A (zh) | 2003-03-19 |
| HK1008229A1 (en) | 1999-05-07 |
| CN1117103C (zh) | 2003-08-06 |
| CN1183787A (zh) | 1998-06-03 |
| BR9608697A (pt) | 1999-07-06 |
| EP0823916B1 (en) | 1999-06-02 |
| EP0823916A1 (en) | 1998-02-18 |
| US5654253A (en) | 1997-08-05 |
| EP0842698A3 (en) | 2001-01-17 |
| AU5548796A (en) | 1996-11-21 |
| CO4560454A1 (es) | 1998-02-10 |
| AU703098B2 (en) | 1999-03-18 |
| CA2217207A1 (en) | 1996-11-07 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US5654253A (en) | Process for hydrogenating aromatic polymers | |
| EP1240211B1 (en) | A process for hydrogenating unsaturated polymers | |
| US5028665A (en) | Polymer hydrogenation catalysts | |
| ES2232509T3 (es) | Procedimiento para hidrogenar polimeros aromaticos. | |
| EP1317492B1 (en) | Improved process for hydrogenating unsaturated polymers | |
| US6172165B1 (en) | Process for hydrogenating aromatic polymers | |
| US6090359A (en) | Process for hydrogenating aromatic polymers | |
| EP1278782B1 (en) | A process for preparing hydrogenated aromatic polymers | |
| HK1008229B (en) | A process for hydrogenating aromatic polymers | |
| US20010051691A1 (en) | Process for preparing hydrogenated aromatic polymers | |
| EP1292627B1 (en) | Hydrogenated monovinylidene aromatic polymer compositions | |
| WO2004029103A1 (en) | Improved process for hydrogenating unsaturated polymers |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 96193724.6 Country of ref document: CN |
|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): AU BR CA CN JP MX SG |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FI FR GB GR IE IT LU MC NL PT SE |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| ENP | Entry into the national phase |
Ref document number: 2217207 Country of ref document: CA Ref document number: 2217207 Country of ref document: CA Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1996912797 Country of ref document: EP |
|
| ENP | Entry into the national phase |
Ref document number: 1996 533327 Country of ref document: JP Kind code of ref document: A |
|
| WWP | Wipo information: published in national office |
Ref document number: 1996912797 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1996912797 Country of ref document: EP |