WO1996033036A1 - Sintering joining method and sintered composite material using same - Google Patents

Sintering joining method and sintered composite material using same Download PDF

Info

Publication number
WO1996033036A1
WO1996033036A1 PCT/JP1996/001061 JP9601061W WO9633036A1 WO 1996033036 A1 WO1996033036 A1 WO 1996033036A1 JP 9601061 W JP9601061 W JP 9601061W WO 9633036 A1 WO9633036 A1 WO 9633036A1
Authority
WO
WIPO (PCT)
Prior art keywords
expansion
based material
copper
iron
sintering
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP1996/001061
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
Takemori Takayama
Yuichi Hori
Hirotaka Kato
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Komatsu Ltd
Original Assignee
Komatsu Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Komatsu Ltd filed Critical Komatsu Ltd
Priority to US08/945,231 priority Critical patent/US5948549A/en
Priority to GB9721626A priority patent/GB2316093B/en
Priority to DE19681350T priority patent/DE19681350C2/de
Publication of WO1996033036A1 publication Critical patent/WO1996033036A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F7/00—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression
    • B22F7/06—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression of composite workpieces or articles from parts, e.g. to form tipped tools
    • B22F7/062—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression of composite workpieces or articles from parts, e.g. to form tipped tools involving the connection or repairing of preformed parts
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B22F3/1039—Sintering only by reaction
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F5/00—Manufacture of workpieces or articles from metallic powder characterised by the special shape of the product
    • B22F5/10—Manufacture of workpieces or articles from metallic powder characterised by the special shape of the product of articles with cavities or holes, not otherwise provided for in the preceding subgroups
    • B22F5/106—Tube or ring forms
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F7/00—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression
    • B22F7/06—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression of composite workpieces or articles from parts, e.g. to form tipped tools
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B23—MACHINE TOOLS; METAL-WORKING NOT OTHERWISE PROVIDED FOR
    • B23K—SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
    • B23K35/00—Rods, electrodes, materials, or media, for use in soldering, welding, or cutting
    • B23K35/001—Interlayers, transition pieces for metallurgical bonding of workpieces
    • B23K35/007—Interlayers, transition pieces for metallurgical bonding of workpieces at least one of the workpieces being of copper or another noble metal
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C1/00—Making non-ferrous alloys
    • C22C1/04—Making non-ferrous alloys by powder metallurgy
    • C22C1/0425—Copper-based alloys
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F2998/00—Supplementary information concerning processes or compositions relating to powder metallurgy
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F2999/00—Aspects linked to processes or compositions used in powder metallurgy
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
    • B22F3/10—Sintering only
    • B22F3/1017—Multiple heating or additional steps
    • B22F3/1028—Controlled cooling
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B22—CASTING; POWDER METALLURGY
    • B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
    • B22F7/00—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression
    • B22F7/06—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression of composite workpieces or articles from parts, e.g. to form tipped tools
    • B22F7/08—Manufacture of composite layers, workpieces, or articles, comprising metallic powder, by sintering the powder, with or without compacting wherein at least one part is obtained by sintering or compression of composite workpieces or articles from parts, e.g. to form tipped tools with one or more parts not made from powder
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C2204/00—End product comprising different layers, coatings or parts of cermet
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00—Stock material or miscellaneous articles
    • Y10T428/12—All metal or with adjacent metals
    • Y10T428/12014—All metal or with adjacent metals having metal particles
    • Y10T428/12028—Composite; i.e., plural, adjacent, spatially distinct metal components [e.g., layers, etc.]
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00—Stock material or miscellaneous articles
    • Y10T428/12—All metal or with adjacent metals
    • Y10T428/12493—Composite; i.e., plural, adjacent, spatially distinct metal components [e.g., layers, joint, etc.]
    • Y10T428/12771—Transition metal-base component
    • Y10T428/12861—Group VIII or IB metal-base component
    • Y10T428/12903—Cu-base component
    • Y10T428/12917—Next to Fe-base component

Definitions

  • the present invention relates to a sintered joining method and a sintered composite member using the method.
  • the present invention relates to a sinter joining method and a sintered composite member using the method, and more particularly to a sinter joining method for sinter joining a copper-based material to an iron-based material and a sinter joining member using the method. Things. Background art
  • a copper pipe material is inserted or press-fitted into the hole and heated, and diffusion bonding is performed using the difference in thermal expansion between the iron material and the copper pipe material and the transformation shrinkage of iron.
  • the methods (1) and (3) described above require the following: (i) If the inner diameter and surface roughness of the hole in the iron-based material and the outer diameter and surface roughness of the copper-based pipe material are not precisely controlled, the joining rate at the joint surface will increase. There are problems such as large variations, a high product rejection rate, a high use for such management, and (ii) the materials used for forming the copper-based pipe material are limited, and the forming is tedious. There is also a method in which a cylindrical copper-based material is press-fitted into a hole of a cylindrical iron-based material and the whole is heated to perform sinter bonding.
  • the present invention has been made in order to solve such a problem, and it is possible to obtain high joining quality without extra cost when sintering a copper-based material to an iron-based material.
  • the object of the present invention is to provide a sinterable joining method and a sintered composite material using the method.
  • the sinter joining method according to the present invention is a sinter joining method for sinter joining a copper-based material to an iron-based material in order to achieve the above-described object.
  • the pot-based material is brought into contact with the iron-based material and heated at a temperature of 600 or more for a predetermined time to expand the copper-based material and join the copper-based material to the iron-based material;
  • the joint strength is further increased by further increasing the temperature and heating at 800 or above, and the material of the punishment is densified.
  • the copper-based material is sufficiently bonded to the iron-based material by heating at a temperature of 600 or more at which the copper-based material exhibits expansion behavior for a predetermined time. Therefore, after that, even if the ⁇ -based material is densified by sintering over 800 t £ l, the copper-based material shifts on the surface of the iron-based material due to shrinkage, and Excellent bonding quality is ensured without separation from Thus, the firing according to the present invention Since the joining method of the copper-based material to the iron-based material is performed only by the temperature control, there is no need for the joining method.
  • the iron-based material is a cylindrical iron-based member, and the copper-based material has an outer diameter substantially equal to or slightly smaller than the inner diameter of the cylindrical iron-based member. It is a copper-based member, and can be heated at a temperature of 60 Ot or more as described above in a state where the cylindrical copper-based member is inserted into the cylindrical iron-based member. By doing so, the cylindrical copper-based member can be joined to the inside of the cylindrical iron-based member.
  • the copper-based material includes a Cu—Sn alloy, and an element stabilizing a phase or a phase similar to the phase of the Cu—Sn alloy is added. It can be.
  • the addition of such an element promotes the expansion behavior of the steel-based material, and the bonding of the copper-based material to the iron-based material becomes stronger.
  • Elements that stabilize such a ⁇ phase or a phase similar to a phase include, for example, A, Si, Ga, Be, In, Sb, Zn, Ti, Zr, F e, N i, M n, C r, C o, one or more of them are used (in addition, the stabilization of an element which stabilizes the same phase as the 9 phase or /?
  • an element that inhibits the chemical function of the copper-based material when the copper-based material is heated to a predetermined temperature exceeding 80 Ot or more is preferable to add an element that inhibits the chemical function of the copper-based material when the copper-based material is heated to a predetermined temperature exceeding 80 Ot or more.
  • the purpose of this element is to promote the densification by changing from a state of expansion behavior to a state of contraction behavior due to sintering. , Zn, P, Sb, Ag, In, or one or more of them.
  • the present invention also relates to a sintered composite member obtained by sintering a copper-based material to an iron-based material by the sintering bonding method according to the present invention as described above. is there.
  • FIG. 1 is a side cross-sectional view showing a test piece of an example
  • FIG. 2 is a graph showing the expansion and contraction behavior of the test specimen of the example
  • FIG. 3 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 4 is a graph showing the expansion and contraction behavior of the test specimen of the example.
  • FIG. 5 is a graph showing the expansion and contraction behavior of the test piece of the example.
  • FIG. 6 is a graph showing the expansion / shrinkage behavior of the test piece of the example.
  • FIG. 7 is a graph showing the expansion and contraction behavior of the test piece of the example.
  • FIG. 8 is a graph showing the expansion and contraction behavior of the test piece of the example.
  • FIG. 9 is a graph showing the expansion and contraction behavior of the test specimen of the example.
  • FIG. 10 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 11 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 12 is an expansion and contraction behavior of the test piece of the example
  • Fig. 13 is a graph showing the expansion and contraction behavior of the test piece of the example
  • Fig. 14 is a graph showing the expansion and contraction behavior of the test piece of the example
  • Fig. 15 is a test piece of the example.
  • Fig. 16 is a graph showing the expansion and contraction behavior of the test piece of the example
  • Fig. 17 is a graph showing the expansion and contraction behavior of the test piece of the example
  • Fig. 18 is a graph showing the expansion and contraction behavior of the test piece.
  • FIG. 19 is a graph showing the expansion / contraction behavior of the test specimen of the example
  • FIG. 19 is a graph showing the expansion / contraction behavior of the test specimen of the example
  • FIG. 20 is a graph showing the expansion and contraction behavior of the test piece of
  • FIG. 21 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 22 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 23 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 24 is a graph showing the expansion and contraction behavior of the test piece of the example
  • FIG. 25 is an expansion and contraction behavior of the test piece of the example.
  • FIG. 26 is a graph illustrating the appearance of the ⁇ phase
  • Figure 27 is a graph showing the required expansion
  • FIG. 28 is a graph illustrating the principle of the present invention. BEST MODE FOR CARRYING OUT THE INVENTION
  • Electrolytic Cu powder (CE 15) was mixed with Cu 20 Sn, Sn atomized powder, TiH, Pb atomized powder, Cu 8 P, graphite in the proportion (wt%) shown in Table 1.
  • Li down iron (2 7% P) prepared S i 0 2, a 1 2 0 3.
  • Z r 02, S ia N *, ⁇ mixed powder was added to and mixed with the powder additive S i C I do.
  • a pressure of 4 t / cm 2 was applied to these mixed powders, and the outer diameter was 25.0 (+0.0, -0.05) mm, the outer diameter was 20, as shown in Fig. 1 (a).
  • Form a thin cylindrical molded body (cylindrical copper-based member) with a thickness of 20 mm.
  • a bottomed cylindrical body (cylindrical shape) made of SCM44OH with an outer diameter of 25.0 (+0.2, —0.0) mm and a depth of 25 mm (Iron-based member).
  • the thin-walled cylindrical molded body was press-fitted into the bottomed cylindrical body, and the dew point was -50, and the temperature was increased in 5 minutes at a heating rate of 5 minutes under an ammonia decomposition gas atmosphere. After holding for a minute, the mixture is cooled at a speed of 30 minutes or more at 30 to obtain a sintered composite member.
  • table 1
  • Each base composition consisted of 25 wt% Cu20Sn, 5 wt% Sn atomized powder, 5 wt% Pb atomized powder, and the balance of electrolytic Cu powder (CE15).
  • Figure 2 shows the results of measuring the dimensional change rate when the same thin-walled cylindrical molded body as above was molded from the mixed powder obtained by adding the additives and the temperature was increased at 790 and 790.
  • the horizontal axis represents the additive amount (wt%) of the additive
  • the vertical axis represents the dimensional change rate (%).
  • Gr represents graphite, and for example, the expression 2 Ti—1 Gr represents Ti added to 2 wt% graphite and 1 wt% added.
  • those containing these additives those containing 0.5 wt% of TiH are excellent in that the clarity of the thin-walled cylindrical body and the bottomed cylindrical body is almost zero. A bonded state was obtained.
  • the upper limit of the TiH addition amount is preferably about 7.0 wt%.
  • T i forms a compound phase such as T i C with graphite, which inhibits bonding, even for iron oxide, which precipitates graphite, from the viewpoint of securing stable bondability and guaranteeing bond strength.
  • the addition amount is preferably 0.2 wt% or more.
  • the lack of expansion on the low temperature side can be sufficiently adjusted by the complex addition of A 1, S i, and Zn described later.
  • the addition of Ti in an amount of 0.2 wt% or more can completely stop the foaming phenomenon during sintering of the Cu—Sn base alloy. Addition effect of CC u 8 p]
  • the addition of P by the Cu-P alloy has a remarkable effect from 0.1 wt% or more.This is thought to be because the fluidity and wettability of a small amount of generated liquid phase are significantly improved. However, since adding a large amount leads to increasing the brittleness of the sintered material, it is preferable to keep the maximum amount to about 1.0 wt%.
  • Mo and W also show significant shrinkage when added alone, and convert to a system that exhibits remarkable swelling properties when added in combination with TiH, so they are also worth studying.
  • the electrolytic Cu powder (CE15) was mixed with the Cu20 Sn, Sn atomized powder, TiH, Pb atomized powder, Si stambu powder, with the composition (wt%) shown in Table 2.
  • a 1 A Tomaizu powder, n i A l stamp flour, n i 2 A 1 3 stamp flour, F el OA l A Tomaizu powder, C u 3 0 Z n A Thomas i's powder, carbonyl n i, carbonyl C Add powder additives such as o, Mo, W, TiSi stam powder, Mn stamp powder, and Cr stamp powder to prepare a copper-based mixed powder.
  • S i, A 1 exhibits expandability is considered to be to stabilize the phase of the Cu—Sn system more, and the state diagram also shows that Cu—S i, Cu—A This signifies that in system 1, the peritectic temperature is on the higher temperature side. It is also considered that TiH is to further stabilize the ⁇ phase of the Cu-Sn system on the low temperature side.
  • the lower limit of the addition amount of T i is set to about 0.2 wt.
  • the reason for this is that the effect of T i can be enhanced by controlling a small amount of S i, A 1 or an intermetallic compound containing these S i, A 1 elements.
  • the expansion from the low-temperature side to the remarkable shrinkage on the high-temperature side was added. You can see that there is.
  • the lower limit of the added amount of Si, A 1 is 0.1 ⁇ ⁇ 1%.
  • the reason for this is that the effect of adding an intermetallic compound containing the Si, A1 or Si, A1 element is remarkable, and the action is sufficiently confirmed.
  • the upper limit ⁇ is preferably 3.0%. The reason for this is that the generation of expansion beyond the required amount requires excessive shrinkage at the high temperature side, making it too difficult to densify.
  • A1 When A1 is added with pure metal powder, it is susceptible to the influence of the sintering atmosphere (oxidation), and may expand excessively on the low-temperature side, making it impossible to achieve high-density on the high-temperature side.
  • A1 can be supplied by a thermally stable intermetallic compound such as NiAl, FeAl or the like. According to this idea, not only the refractory intermetallic compound between Ni—Al and Fe—A1 but also the Cu—A and Ni—Mn-A1 and Co— close to the Ni and Fe groups. A similar effect can be expected for the intermetallic compound between A and Cr-A 1. Conceivable. Therefore, the addition of these intermetallic compounds is also consistent with the gist of the present invention. The amount of A1 is converted by the A1 content of the intermetallic compound, and the contents of Ni, Fe, Co, Cr, and Mn contained simultaneously are included in the scope of the present invention. is there.
  • FIGS. 7 and 8 show the effect of adding Sn and Pb on Cu — 6 Ti. From these effects, it is considered that the lower limit of the amount of Sn added is about 2 wt%. It can be seen that if Pb is added at 10 wt%, shrinkage on the high temperature side can be ensured. However, considering the bondability with iron (expansion of expandability of S i and A 1), the amount of Sn added is considered. About 2 wt% is considered necessary. FIG.
  • the result of measuring the dimensional shrinkage by adding the additive in another mode is shown in the graph of FIG. From the graphs of Figs. 12, 13, 14 and 15 and 16, the coexistence effect of Ni and Ti is not so remarkable when the amount of TiH added is small. It can be seen that it exerts the effect of suppressing shrinkage on the low-temperature side, contributing to the stabilization of the joint, and accelerates the densification on the high-temperature side. Further, N i, coexistence effect of T i is markedly increase bonding strength at the interface ⁇ of the bottomed cylindrical member, for example, 2 0 ⁇ 2 5 kg / mm 2 and prominent in shear strength in the example of C 2 in Table 4 It can be seen that a great effect is exhibited. Furthermore, favorable results can be obtained by increasing the amounts of Ni and TiH added (FIGS. 13 and 14). These effects have been observed for Co as well.
  • the amount of Ti H added is 3 wt%.
  • An upper limit may be set for the degree.
  • the addition amount may be set to a lower limit of about 0.5 wt%, since the effect can be recognized by adding 5 times the addition amount of Si and A 1. Also, from the viewpoint of cost, it is conceivable to set an upper limit of about 2 Owt%. In order to obtain a sufficiently stable effect, it is considered that about 2 to 5 wt% is preferable.
  • the lower limit of the amount of Zn added is, for example, when the effect of coexistence of 0.5 wt% A 1 is observed, the low-temperature expansion is proportional to the amount of added Zn. However, it is thought that it can be set to 0 wt% because it becomes remarkable.
  • the upper limit of the amount of Zn added can be set to about 30 ⁇ / ⁇ 1% from the viewpoint of the difficulty in formability when Zn is added as a master alloy.
  • the influence of the amount of addition leads to the adjustment of the expansion temperature depending on the amount of addition, so that the addition source of Sn, Pb, TiH, etc. It can be easily adjusted by adding and subtracting elements.
  • sintering is performed in a pressurized atmosphere of an inert gas such as N 2 gas or a reducing gas in consideration of the evaporation of Zn. This is considered to be effective in increasing the sintering density on the high temperature side.
  • a thick solid line indicates the thermal expansion / shrinkage curve of ⁇ (SCM440 0) (1), and the outside of the thin cylindrical molded body (Cu-based pipe molding material) Clearance between the diameter and the inner diameter of the bottomed cylinder (0 2 The thermal expansion and shrinkage curves of ⁇ when expected to be 50 ⁇ m for 5 mm) are shown by another thick solid line.
  • Cu—33Sn is a good source of Sn and a Cu—20Sn source has a large amount of Cu20Sn powder added.
  • the shrinkage due to the reaction cannot be ignored, and the appearance of a new / 9 phase above the peritectic point of the Cu-Sn system is hardly expected, so that the expansion required for bonding cannot be expected. I understand.
  • sintering is performed by heating to a temperature at which the copper powder material is sufficiently densified (preferably at a relative density of 85% or more) in accordance with the composition of each copper-based powder material.
  • the gist of the present invention is to make the expansion on the high temperature side which is easy to use for joining appear.
  • the liquid phase and the new appearance of the phase necessary for joining are expressed by making full use of the alloy design technique and used for joining.
  • the expansion amount due to the addition of the alloy element expands by 0.5% compared to the base alloy, and when the clearance is expected to be 50 m, it is about 0 (for ⁇ 25 mm). If the expansion is 8%, it is considered that the joint can be formed. The reason for this is in good agreement with the above results, but considering the stability of the joint and the safety against process variations, it is advisable to secure at least 1% expansion relative to the base. It is possible.
  • the amount of carbon changes for example, the amount of carbon changes, the transformation point of ⁇ changes.
  • A, S i, G a, B e, I n, S b, and Z n systems are selected as those that meet the above-mentioned gist.
  • a 1 is most effective if it has a phase stabilizing effect, and S i and Z n are also practical. It is convenient as a realistic alloy element.
  • the method of adding AI, Si, and Zn Since the precipitation of the phase due to the reaction with the liquid phase that occurs during the sintering is considered to be the basis of the expansion reaction, the same effect is exhibited even if the expansion element is a compound such as NiA1 or a method of adding a master alloy. It is easy to imagine.
  • G a, B e, In and S b are also considered to basically exhibit the same effects as Al, S i and In.
  • the condition of the element that stabilizes the ⁇ phase by adding it as an alloy element is that the crystal structure of the alloy element is The element must have at least the same BCC structure as the ⁇ phase and be capable of solid solution of Cu to some extent
  • T i, Z r, and F e are selected as those that meet such a gist.
  • the effect as an expansion element is considered to be smaller than that of the element (1).
  • Addition of the expansion element makes it difficult for the density of the sintered body to increase even in the high-temperature region and increases the inconvenience in the material properties.Therefore, adjust the sintering density to be low within the specified temperature range. Need to be done.
  • the function as an element that promotes high densification is to change the precipitate morphology so that the expansion element, for example, the / 9 phase stabilization function of S i, A 1 is suppressed at 850 above.
  • the expansion element for example, the / 9 phase stabilization function of S i, A 1 is suppressed at 850 above.
  • 9 ⁇ Ni 3 Si, Ti A 1, Ni 3 Ti, Ti Si, C ⁇ Ti C, etc. can be considered.
  • one gist of the present invention is that, as schematically shown in the graph of FIG. 28, the impregnated material is expanded at the lower sintering temperature and pressed against the iron-based material.
  • the sintering is performed at the high sintering temperature to obtain the required compactness as a sintered material.
  • the bonding property can be improved by slowing down the rate of temperature rise in the sintering on the low temperature side or by heating at the same temperature for a predetermined time in the temperature range on the low temperature side.
  • the copper-based material is simply brought into contact with the iron-based material without being pressed into contact with the iron-based material for sintering. In this case, when joining the ferrous material to the ferrous material by sintering on the low temperature side, the copper material does not deviate from the ferrous material in an unexpected direction due to shrinkage Benefit.
  • the sinter joining method of the present invention and the sintered composite member obtained by the method are applied to, for example, a cylinder block.

Landscapes

  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Chemical & Material Sciences (AREA)
  • Materials Engineering (AREA)
  • Manufacturing & Machinery (AREA)
  • Composite Materials (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Powder Metallurgy (AREA)
PCT/JP1996/001061 1995-04-19 1996-04-19 Sintering joining method and sintered composite material using same Ceased WO1996033036A1 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
US08/945,231 US5948549A (en) 1995-04-19 1996-04-19 Sinter joining method and sintered composite member produced by same
GB9721626A GB2316093B (en) 1995-04-19 1996-04-19 Sinter joining method and sintered composite member produced by same
DE19681350T DE19681350C2 (de) 1995-04-19 1996-04-19 Sinter-Verbindungsverfahren und damit hergestelltes gesintertes Verbundelement

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP7/93977 1995-04-19
JP7093977A JP3045460B2 (ja) 1995-04-19 1995-04-19 焼結接合方法およびその方法を用いる焼結複合部材

Publications (1)

Publication Number Publication Date
WO1996033036A1 true WO1996033036A1 (en) 1996-10-24

Family

ID=14097469

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP1996/001061 Ceased WO1996033036A1 (en) 1995-04-19 1996-04-19 Sintering joining method and sintered composite material using same

Country Status (6)

Country Link
US (1) US5948549A (enExample)
JP (1) JP3045460B2 (enExample)
KR (1) KR100200267B1 (enExample)
DE (1) DE19681350C2 (enExample)
GB (1) GB2316093B (enExample)
WO (1) WO1996033036A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2002044127A1 (fr) * 2000-11-29 2002-06-06 Kyorin Pharmaceutical Co., Ltd. Dérivés d'acide carboxylique substitué

Families Citing this family (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3859344B2 (ja) 1998-01-28 2006-12-20 株式会社小松製作所 摺動材料,摺動部材およびその摺動部材の製造方法
JP2003089831A (ja) * 2001-07-12 2003-03-28 Komatsu Ltd 銅系焼結摺動材料および複層焼結摺動部材
ITBO20030668A1 (it) * 2003-11-12 2005-05-13 R C M Italiana S R L Procedimento per la produzione di boccole d'acciaio e/o d'altro adatto metallo, con un rivestimento interno e/od esterno di materiale a basso coefficiente d'attrito, ad esempio per la produzione di boccole composite
JP4849462B2 (ja) * 2006-11-15 2012-01-11 日立粉末冶金株式会社 複合焼結機械部品の製造方法およびシリンダブロック
JP4545162B2 (ja) * 2007-02-19 2010-09-15 株式会社小松製作所 複合焼結摺動部材とその製造方法
DE102016103752A1 (de) 2015-03-06 2016-09-08 Gkn Sinter Metals, Llc Verfahren zur Herstellung eines Messing oder Bronze aufweisenden Verbundbauteils mittels Sinterpassung
CN111405955B (zh) * 2017-11-28 2022-03-22 日本碍子株式会社 导电性前端构件及其制造方法
DE102018212625A1 (de) * 2018-07-27 2020-01-30 Rolls-Royce Deutschland Ltd & Co Kg Verfahren zur Herstellung eines Bauteils unter Verwendung eines Sinterfügeprozesses
DE102021115936A1 (de) 2020-07-08 2022-01-13 Transportation Ip Holdings, Llc Kolbenkühldüse
DE102021116316A1 (de) 2020-07-08 2022-01-13 Transportation Ip Holdings, Llc Verfahren und system zur fertigung von ausrüstung
USD965029S1 (en) 2020-09-11 2022-09-27 Transportation Ip Holdings, Llc Piston cooling jet

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS57101603A (en) * 1980-12-16 1982-06-24 Oiles Ind Co Ltd Sintered sliding component comprising plural layers and preparation thereof
JPS61179804A (ja) * 1985-01-09 1986-08-12 Mitsubishi Metal Corp 鉄系焼結体と銅系焼結体の接合品の製造方法
JPH01198407A (ja) * 1988-02-03 1989-08-10 Oiles Ind Co Ltd 鋳鉄製裏金を有する複層焼結摺動部材

Family Cites Families (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US628427A (en) * 1898-10-21 1899-07-04 Copper And Steel Welding Company Welding metals.
US2482898A (en) * 1941-06-23 1949-09-27 Metals & Controls Corp Corrosion-resisting composite metal
US3282660A (en) * 1964-03-26 1966-11-01 Anaconda Wire & Cable Co High-temperature electrical conductor and method of making
US3397445A (en) * 1965-09-30 1968-08-20 Ulmer Method of making bimetal tubing
US4505987A (en) * 1981-11-10 1985-03-19 Oiles Industry Co., Ltd. Sliding member
CH660882A5 (de) * 1982-02-05 1987-05-29 Bbc Brown Boveri & Cie Werkstoff mit zweiweg-gedaechtniseffekt und verfahren zu dessen herstellung.
JPS59205105A (ja) * 1983-05-07 1984-11-20 住友電気工業株式会社 導電性複合材料
JPS644406A (ja) * 1987-06-26 1989-01-09 オイレス工業株式会社 複層からなる焼結摺動部材の製造方法
JPH0336203A (ja) * 1989-06-29 1991-02-15 Komatsu Ltd 二重構造のシリンダブロックの製造方法
JPH0578711A (ja) * 1991-09-20 1993-03-30 Tokico Ltd 径方向に非円形穴を有する筒状部材の製造方法

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS57101603A (en) * 1980-12-16 1982-06-24 Oiles Ind Co Ltd Sintered sliding component comprising plural layers and preparation thereof
JPS61179804A (ja) * 1985-01-09 1986-08-12 Mitsubishi Metal Corp 鉄系焼結体と銅系焼結体の接合品の製造方法
JPH01198407A (ja) * 1988-02-03 1989-08-10 Oiles Ind Co Ltd 鋳鉄製裏金を有する複層焼結摺動部材

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2002044127A1 (fr) * 2000-11-29 2002-06-06 Kyorin Pharmaceutical Co., Ltd. Dérivés d'acide carboxylique substitué

Also Published As

Publication number Publication date
US5948549A (en) 1999-09-07
JPH08291306A (ja) 1996-11-05
JP3045460B2 (ja) 2000-05-29
DE19681350T1 (de) 1998-04-02
GB2316093A (en) 1998-02-18
KR960037185A (ko) 1996-11-19
DE19681350C2 (de) 2001-06-13
GB2316093B (en) 1999-05-26
GB9721626D0 (en) 1997-12-10
KR100200267B1 (ko) 1999-06-15

Similar Documents

Publication Publication Date Title
US5509555A (en) Method for producing an article by pressureless reactive infiltration
JPH0617524B2 (ja) マグネシウム―チタン系焼結合金およびその製造方法
JP3045460B2 (ja) 焼結接合方法およびその方法を用いる焼結複合部材
Walker et al. Selective laser sintering of composite copper–tin powders
US5269830A (en) Process for synthesizing compounds from elemental powders and product
JP5987000B2 (ja) 高熱伝導性を有するアルミニウム合金粉末金属
JP5962787B2 (ja) 粉末冶金用混合粉およびその製造方法ならびに鉄基粉末製焼結体
JPH08291306A5 (enExample)
JPH02153063A (ja) 窒素強化合金の製造方法
TW573016B (en) Processing of iron aluminides by pressureless sintering of elemental iron and aluminum
JP5962691B2 (ja) 粉末冶金用混合粉およびその製造方法ならびに鉄基粉末製焼結体
US8802004B2 (en) Component produced or processed by powder metallurgy, and process for producing it
JPH0639605B2 (ja) 鋳鉄製裏金を有する複層焼結摺動部材
US6096111A (en) Exothermically sintered homogeneous composite and fabrication method
CN103182503B (zh) Cu系熔渗用粉末
JP6380501B2 (ja) 粉末冶金用混合粉、粉末冶金用混合粉の製造方法、および焼結体
CN112719272B (zh) 一种增材制造高熵合金齿轮的方法
JP6007928B2 (ja) 粉末冶金用混合粉およびその製造方法ならびに鉄基粉末製焼結体
US20100015463A1 (en) Three-part metallurgy system including aluminum and titanium for lightweight alloy
JP2020037735A (ja) 合金粉末組成物
Novák et al. Effect of alloying elements on microstructure and properties of Fe-Al and Fe-Al-Si alloys produced by reactive sintering
JP3578409B2 (ja) 焼結摺動部材の製造方法
CN119794332A (zh) FeSi-Ni3Si/TiB2-TiC复合材料及其熔融金属液相烧结工艺
JPH03229832A (ja) Nb―Al金属間化合物の製造方法
JPH0543996A (ja) 焼結摺動部材ならびにその製造方法

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): DE GB US

DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
WWE Wipo information: entry into national phase

Ref document number: 08945231

Country of ref document: US

RET De translation (de og part 6b)

Ref document number: 19681350

Country of ref document: DE

Date of ref document: 19980402

WWE Wipo information: entry into national phase

Ref document number: 19681350

Country of ref document: DE