WO1995022577A1 - Polyamides having improved color and processibility and process for manufacturing - Google Patents
Polyamides having improved color and processibility and process for manufacturing Download PDFInfo
- Publication number
- WO1995022577A1 WO1995022577A1 PCT/US1995/001950 US9501950W WO9522577A1 WO 1995022577 A1 WO1995022577 A1 WO 1995022577A1 US 9501950 W US9501950 W US 9501950W WO 9522577 A1 WO9522577 A1 WO 9522577A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- polyamide
- phosphorus
- multivalent metal
- group
- polymerization
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K5/00—Use of organic ingredients
- C08K5/49—Phosphorus-containing compounds
- C08K5/51—Phosphorus bound to oxygen
- C08K5/52—Phosphorus bound to oxygen only
- C08K5/524—Esters of phosphorous acids, e.g. of H3PO3
- C08K5/526—Esters of phosphorous acids, e.g. of H3PO3 with hydroxyaryl compounds
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G69/00—Macromolecular compounds obtained by reactions forming a carboxylic amide link in the main chain of the macromolecule
- C08G69/02—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids
- C08G69/26—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids derived from polyamines and polycarboxylic acids
- C08G69/28—Preparatory processes
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K13/00—Use of mixtures of ingredients not covered by one single of the preceding main groups, each of these compounds being essential
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K3/00—Use of inorganic substances as compounding ingredients
- C08K3/16—Halogen-containing compounds
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K3/00—Use of inorganic substances as compounding ingredients
- C08K3/32—Phosphorus-containing compounds
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K5/00—Use of organic ingredients
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K5/00—Use of organic ingredients
- C08K5/04—Oxygen-containing compounds
- C08K5/09—Carboxylic acids; Metal salts thereof; Anhydrides thereof
- C08K5/095—Carboxylic acids containing halogens
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K5/00—Use of organic ingredients
- C08K5/49—Phosphorus-containing compounds
- C08K5/51—Phosphorus bound to oxygen
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K5/00—Use of organic ingredients
- C08K5/49—Phosphorus-containing compounds
- C08K5/51—Phosphorus bound to oxygen
- C08K5/52—Phosphorus bound to oxygen only
- C08K5/524—Esters of phosphorous acids, e.g. of H3PO3
Definitions
- This invention relates to polyamide resins having improved color and processibility and a process for manufacturing these resins.
- the polyamide resins prepared in accordance with the process of the present invention are particularly useful in molding and extrusion applications and are manufactured in the presence of certain phosphorus compounds in conjunction with certain multivalent metal compounds.
- An object of the present invention is to provide polyamide resins which initially appear less yellow than the same resins having not been manufactured in accordance with the present invention.
- a further object of the present invention is to provide polyamide resins which undergo a lesser degree of color build-up (i.e., increase in yellowness) on storage as compared to the same resins having not been manufactured in accordance with the present invention.
- an object of the present invention is to provide polyamide resins which do not undergo significant molecular weight increases during subsequent melt processing operations. It is generally known that when polyamide resins are manufactured according to conventionally known processes without the addition of conventional pigments, these resins tend to exhibit varying degrees of yellowness in initial color, with said yellowness increasing over time.
- the resins also generally exhibit increased yellowness when exposed to high temperatures during subsequent melt processing operations. For example, during molding and extrusion applications, a certain amount of the resin is subjected to repeated melting in the form of regrind, which generally results in the molded or extruded resin exhibiting increased yellowness. Therefore, considering the extended storage time for some of these resins and the repeated melting during molding and extrusion, there exists a need to provide a process for manufacturing improved polyamide resins which initially appear, and continue to appear over time, less yellow than the same resins not prepared in accordance with the present invention. Polyamide resins and their preparation are well known in the art.
- dicarboxylic acids include, for example, adipic acid, azelaic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid, isophthalic acid, and terephthalic acid
- representative diamines include, for example, hexamethylenediamine, octamethylenediamine, tetramethylenediamine, 2- methylpentamethylenediamine, decamethylenediamine, and dodecamethylenediamine.
- Representative amino acids include 6- aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.
- polyamide-forming reactants the above-identified compounds shall be referred to as "polyamide-forming reactants" and this term shall include combinations of the compounds, as well as individual compounds, provided the combination or individual compound can be polymerized to form polyamides.
- phosphorus compounds serve as color stabilizers for the polyamides by reducing the degree of oxidative and thermal degradation.
- these phosphorus compounds also serve as polymerization catalysts and in addition, some serve as nucleating agents, as in U.S. Patent No. 4,237,034.
- Nucleated polyamides generally have lower toughness compared to polyamides which have not been nucleated and thus, phosphorus compounds which function as nucleating agents are not particularly desirable in applications where a loss in toughness is not desired.
- the catalytic effect of certain phosphorus compounds on a polyamide polymerization process can be reduced or stopped completely by the addition therein of certain multivalent metal compounds without significantly and adversely affecting the phosphorus compound's desired effect of reducing resin color.
- the degree to which the phosphorus compound, acting as a catalyst, is deactivated depends on the amounts of phosphorus and multivalent metal compound added to the polymerization process or to the polyamide melt. For economical and efficient processing, some degree of catalytic effect is desired for increased throughput, especially when polymerization is conducted by a continuous mode process, which is, generally, a kinetically limited process.
- polyamide resins made by the process herein are useful in numerous molding applications (i.e., automobile parts, mechanical parts, electrical and electronic parts, molded gears, sports equipment, appliances, etc.) and extrusion applications (i.e., tubing, rods, filaments, films, etc.).
- the present invention relates to a process for manufacturing polyamide resins, said resins being particularly useful in molding and extrusion applications.
- the polyamide resins prepared in accordance with the process of the present invention exhibit improved initial color (i.e., reduced yellowness) and color stability on storage. Furthermore, the polyamide resins prepared in accordance with the process of the present invention do not undergo significant molecular weight increases during subsequent melt processing operations.
- the process of the present invention comprises polymerizing poly amide-forming reactants in the presence of certain phosphorus compounds in conjunction with certain multivalent metal compounds.
- the process of the present invention comprises compounding into a polyamide melt certain phosphorus compounds in conjunction with certain multivalent metal compounds.
- Polymerization processes are well known and can be, for example, batch or continuous mode processes.
- the polymerization processes contemplated by the present invention are those processes generally used to manufacture well known polyamides, such as nylons 6, 11, 12, 66, 69, 610, 612, and their copolymers from well known polyamide-forming reactants.
- the preferred polyamide-forming reactants to be used in the process of the present invention are those polyamide-forming reactants generally used to manufacture nylons 6, 66, 610 and 612.
- the phosphorus compounds used in the process of the present invention, and their preparation, are well known in the art. These phosphorus compounds serve as color stabilizers and polymerization catalysts in nylons. They include phosphorous acids, their salts, and their organic esters. Examples of the phosphorous acids include hypophosphorous acid, orthophosphorous acid, pyrophosphorous acid, and diphosphorous acid.
- the phosphorous acid salts useful in the present invention include salts of Groups IA and IIA, manganese, zinc, aluminum, ammonia, and alkyl or cycloalkyl amines or diamines. Examples of the organic esters useful in the present invention include mono-, di-, and triesters of phosphorous acid.
- the organic esters useful in the process of the present invention do not have direct carbon-phosphorus bonds so that in the presence of water, said esters undergo hydrolysis and are converted to inorganic phosphorus acids or their salts. Hydrolysis of phosphorus esters containing carbon-phosphorus linkage produces organophosphorous acids or their salts. Metal salts of these organophosphorous acids generally act as nucleating agents in nylons (U.S. 4,237,034), which can result in an undesirable reduction in polymer toughness.
- the preferred phosphorus compounds for use in the process of the present invention are hypophosphorous acid, orthophosphorous acid, diphosphorous acid, and their respective salts. Sodium hypophosphite (SHP) is the most preferred phosphorus compound.
- the above-described phosphorus compounds are added in an amount sufficient to constitute concentrations ranging from 0.097 to 1.582 mols phosphorus (in the phosphorus compound) per million grams polyamide, preferably from 0.194 to 1.129 mols phosphorus (in the phosphorus compound) per million grams polyamide.
- the phosphorus compound can be introduced at any point prior to, during, or after polymerization, it is preferable to add the phosphorus compound as early as possible (i.e., pre-polymerization). If added after polymerization, then initial color will not be improved but color stability during subsequent storage or processing will be improved.
- the multivalent metal compounds used in the present invention serve as phosphorus catalyst deactivators, thereby significantly reducing any undesirable increase in the molecular weight of the polyamide during subsequent melt processing operations.
- the degree of phosphorus catalyst deactivation may be controlled by the amount of the phosphorus compound and the multivalent metal compound added to the polyamide.
- the multivalent metal compound is introduced into the polymerization process, or alternatively into the polyamide melt, in an amount ranging from about 0.097 mol to about 50 mols multivalent metal compound per million grams polyamide, preferably from about 0.150 mol to about 5 mols multivalent metal pound per million grams polyamide.
- the multivalent metal compounds useful in the present invention are well known to one skilled in the art and include halides, nitrates, and carboxylate salts (i.e., acetates, proprionates, benzoates, stearates, etc.) of Group IIA metals, zinc and aluminum.
- the preparation of polyamides by polymerization processes can occur by generally known methods, such as a batch method or a continuous mode method.
- a conventional batch method typically a 40-60% polyamide salt solution formed from equimolar amounts of diacid and diamine in water, is charged into a preevaporator vessel operated at a temperature of about 130-160°C and a pressure of about 35-100 psia, wherein the polyamide salt solution is concentrated to about 70-80%.
- the concentrated solution is then transferred to an autoclave, wherein heating is continued as the pressure in the vessel rises to about 160-600 psia, generally 195-300 psia.
- the phosphorus compound and the multivalent metal compound can be added before polymerization (i.e., into a solution of at least one polyamide-forming reactant), or can be introduced at any point during polymerization, or can even be introduced post- polymerization (i.e., by incorporating the phosphorus compound and the multivalent metal compound into a polyamide melt, using conventional mixing equipment, such as an extruder).
- the phosphorus compound and multivalent metal compound can be introduced separately or all at once.
- the phosphorus compound and the multivalent metal compound should be added as early as possible in the polymerization process, preferably at the beginning of the polymerization process. Additionally, they can be added in solid form or in the form of aqueous solutions.
- Continuous polymerizations are also well known in the art (See U.S. Patent 3,947,424).
- the polyamide salt solution is preheated in a preheater vessel to about 40-90°C, then transferred into a pre- evaporator/reactor where the salt solution is concentrated at about 195-300 psia and about 200-260°C to about 70-90%, resulting in a low molecular weight polymer.
- the low molecular weight polymer is then discharged into a flasher, where the pressure is slowly reduced to below 15 psia and then discharged into a vessel maintained below atmospheric pressure and at a temperature of about 270-300°C to effect removal of water and to promote further molecular weight increase.
- the polyamide melt is then extruded into a strand, cooled, and cut into pellets.
- the phosphorus compound and multivalent metal compound can be incorporated at any point during the process, including post-polymerization (i.e., by compounding them into the polyamide melt, etc.). However, for maximum antioxidant and thermal protection, and for optimum catalyst deactivation, it is recommended that the phosphorus compounds and multivalent metal compounds be added prior to polymerization or as early as possible. Additionally, it is understood that the polyamides prepared by the process of the present invention may also contain conventional additives such as pigments and dyes, flame retardants, lubricants, optical brighteners, organic antioxidants, plasticizers, heat stabilizers, ultraviolet light stabilizers, nucleating agents, tougheners, and reinforcing agents.
- conventional additives such as pigments and dyes, flame retardants, lubricants, optical brighteners, organic antioxidants, plasticizers, heat stabilizers, ultraviolet light stabilizers, nucleating agents, tougheners, and reinforcing agents.
- the resins in the following were analyzed for molecular weight (RV), as measured in accordance with ASTM D789, and Yellowness Index (YI), as measured in accordance with ASTM D 1925 using a Hunter
- YI is a measure of the degree of yellowness exhibited by a resin. The lower the YI value, the less yellow the resin appears.
- Initial RV refers to the molecular weight of the sample before solid phase polymerization at 180°C for 3 hours.
- Frinal RV refers to the molecular weight of the sample after solid phase polymerization at 180°C for 3 hours.
- a nylon 66 salt solution with a pH of 7.45 and nylon salt concentration of about 51.5 weight percent was pumped into a preheater at a rate of 4950 lb/hr, where it was heated from about 41°C to about 55°C.
- the nylon salt solution was then pumped into a prepolymerizer operating at around 235°C and 225 psia, where it was concentrated to about 90% nylon salt, and wherein the monomers were converted to low molecular weight polymer.
- the SHP was added as an aqueous solution to the nylon 66 salt solution. It is noted that in Examples 1-1 to 1-4, all additions of SHP were in the form of aqueous solutions containing a sufficient amount of SHP to yield the desired amount of SHP (in ppm) in the polyamide.
- Example 1-2 was prepared as described above with the addition of 101 ppm of SHP to the nylon salt solution. Additionally, 500 ppm of calcium acetate was added to the nylon melt just before the die.
- Example 1-3 was prepared as described above with the addition of 184 ppm of SHP to the nylon salt solution. Additionally, 850 ppm of calcium acetate was added to the nylon melt just before the die
- Example 1-4 was prepared as described above with the addition of 103 ppm of SHP to the nylon salt solution. Additionally, 1000 ppm of aluminum distearate was added to the nylon melt just before the die YI values for Cl and Examples 1-1 to 1-4 are given in TABLE
- the polymers of Cl and Examples 1-1 to 1-4 were each subjected to solid phase polymerization at 180°C for 3 hours.
- the molecular weights (RV) of the resulting polymers were measured and reported in TABLE III below. Note that after preparation of each example the initial RV was measured before the polymer was subjected to solid phase polymerization. Also shown in TABLE TTT is the increase in molecular weight resulting from the solid phase polymerization. The larger the RV increase, the greater the catalytic effect on polymerization.
- the data reported for Cl shows the normal increase in RV for nylon 66 under the described conditions.
- Example 1-1 illustrates the effect of SHP on polymerization.
- Examples 1-2 to 1-4 show the effect of the multivalent metal compounds on the rate of polymerization.
- the RV increase for Examples 1-2 to 1-4 were comparable to Cl.
- Example 2-1 was prepared the same as C2, with the exception that 109 grams of SHP were dissolved in 1 gallon of demineralized water and this solution was added to the autoclave containing the 80% concentrated nylon salt solution.
- Example 2-2 was prepared the same as C2 with the exception that 109 grams of SHP and 9.2 grams of cobalt aluminate pigment were dissolved in 5 gallons of demineralized water. This suspension (noting that cobalt aluminate pigment does not dissolve in water) was added to the autoclave containing the 80% concentrated nylon salt solution.
- Example 2-2 To analyze the effect of multivalent metal compounds on the catalytic effect of SHP, the polymer of Example 2-2 above was melt blended in a 28 mm Werner & Pfleiderer twin-screw extruder under atmospheric pressure at a temperature of about 280°C to 300°C with various multivalent metal compounds as indicated in TABLE V. The polymer melt was then extruded through a circular die, cooled and cut into pellets. The resulting polymers are listed in TABLE V as Examples 3-1 to 3-6. The compositions are shown in the table.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Polyamides (AREA)
- Compositions Of Macromolecular Compounds (AREA)
Priority Applications (4)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| EP95911758A EP0745106B2 (en) | 1994-02-16 | 1995-02-15 | Process for preparation of polyamides having improved color and processibility |
| JP52190695A JP3504664B2 (ja) | 1994-02-16 | 1995-02-15 | 改良された色および加工性を有するポリアミド並びに製造方法 |
| CA002181236A CA2181236C (en) | 1994-02-16 | 1995-02-15 | Polyamides having improved color and processibility and process for manufacturing |
| DE69500807T DE69500807T3 (de) | 1994-02-16 | 1995-02-15 | Verfahren zur herstellung von polyamiden mit verbesserter färbung und verarbeitung |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US19708394A | 1994-02-16 | 1994-02-16 | |
| US08/197,083 | 1994-02-16 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1995022577A1 true WO1995022577A1 (en) | 1995-08-24 |
Family
ID=22727978
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1995/001950 Ceased WO1995022577A1 (en) | 1994-02-16 | 1995-02-15 | Polyamides having improved color and processibility and process for manufacturing |
Country Status (6)
| Country | Link |
|---|---|
| US (1) | US5929200A (enExample) |
| EP (1) | EP0745106B2 (enExample) |
| JP (1) | JP3504664B2 (enExample) |
| CA (1) | CA2181236C (enExample) |
| DE (1) | DE69500807T3 (enExample) |
| WO (1) | WO1995022577A1 (enExample) |
Cited By (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1997043236A1 (de) * | 1996-05-14 | 1997-11-20 | Rathor Ag | Verfahren zur bromierung natürlicher ungesättigter öle |
| WO1999061522A1 (en) * | 1998-05-29 | 1999-12-02 | Solutia Inc. | Nucleation of polyamides in the presence of hypophosphite |
| EP1036819A4 (en) * | 1998-08-24 | 2001-08-01 | Asahi Chemical Ind | POLYAMIDE RESIN COMPOSITION AND METHOD FOR THE PRODUCTION THEREOF |
| WO2005000953A3 (de) * | 2003-06-27 | 2005-03-17 | Ems Chemie Ag | Polyamidformmasse, verfahren zur herstellung der polyamidformmasse und formteile herstellbar aus der polyamidformmasse |
| US7491763B2 (en) | 2002-07-10 | 2009-02-17 | Asahi Kasei Chemicals Corporation | Polyamide composition |
| WO2015183385A1 (en) * | 2014-05-30 | 2015-12-03 | Ascend Performance Materials Operations Llc | Low phosphorus low color polyamides |
| WO2020132002A1 (en) * | 2018-12-18 | 2020-06-25 | Ascend Performance Materials Operations Llc | Antimicrobial nonwoven polyamides with zinc content |
| WO2020132006A1 (en) * | 2018-12-18 | 2020-06-25 | Ascend Performance Materials Operations Llc | Antimicrobial polymer compositions, fibers, and yarns |
Families Citing this family (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6515058B1 (en) | 2000-08-09 | 2003-02-04 | Asahi Kasei Kogyo Kabushiki Kaisha | Polyamide resin composition |
| FR2818985B1 (fr) * | 2000-12-29 | 2004-02-20 | Nylstar Sa | Procede de fabrication de compositions stabilisees a base de polyamide |
| JP4112459B2 (ja) * | 2002-08-12 | 2008-07-02 | 旭化成ケミカルズ株式会社 | ポリアミド樹脂組成物およびその製造方法 |
| DE10337707A1 (de) * | 2003-08-16 | 2005-04-07 | Degussa Ag | Verfahren zur Erhöhung des Molekulargewichts bei Polyamiden |
| JP4446731B2 (ja) * | 2003-12-25 | 2010-04-07 | 旭化成ケミカルズ株式会社 | ポリアミド66樹脂ペレットの製造方法 |
| JP4480391B2 (ja) * | 2003-12-25 | 2010-06-16 | 旭化成ケミカルズ株式会社 | ポリアミド66樹脂ペレット及びその製造方法 |
| US8501900B2 (en) | 2009-08-10 | 2013-08-06 | Invista North America S.A R.L. | Nylon resins and process |
| JP6822766B2 (ja) | 2015-01-22 | 2021-01-27 | 旭化成株式会社 | ポリアミド樹脂組成物を含む成形体 |
| CN104558587B (zh) * | 2015-01-30 | 2017-07-28 | 江苏弘盛新材料股份有限公司 | 一种光热稳定尼龙6及其制备方法 |
| US10927232B2 (en) | 2015-02-20 | 2021-02-23 | Asahi Kasei Kabushiki Kaisha | Polyamide resin composition, method for producing polyamide resin composition, and molded article |
| KR102656072B1 (ko) | 2018-07-13 | 2024-04-09 | 어센드 퍼포먼스 머티리얼즈 오퍼레이션즈 엘엘씨 | 아연 및 인 함량을 갖는 항균 중합체 수지, 섬유 및 원사 |
| CA3170492A1 (en) * | 2020-03-04 | 2021-09-10 | Vikram Gopal | Antiviral articles |
| CN113980266A (zh) * | 2021-11-30 | 2022-01-28 | 会通新材料(上海)有限公司 | 一种低黄色指数长碳链聚酰胺及其制备方法 |
| EP4594423A1 (en) | 2022-09-27 | 2025-08-06 | Basf Se | Thermoplastic moulding compositions having an improved colour stability-1 |
Citations (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US3384615A (en) * | 1966-05-16 | 1968-05-21 | Grace W R & Co | Stabilization of polyamides |
| US4237034A (en) * | 1973-05-14 | 1980-12-02 | Imperial Chemical Industries Limited | Polyamide compositions containing carboxylic acid metal salt and organophosphonic acid |
Family Cites Families (18)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| BE608862A (enExample) † | 1960-10-06 | 1900-01-01 | ||
| US3173898A (en) † | 1961-03-20 | 1965-03-16 | Du Pont | Polymerization of polyamide-forming reactants with hypophosphite catalysts |
| NL297427A (enExample) † | 1962-09-03 | |||
| DE1495147A1 (de) * | 1963-10-18 | 1969-01-30 | Basf Ag | Verfahren zum Herstellen von Polylaurinlactam |
| AT251883B (de) * | 1963-12-13 | 1967-01-25 | Snia Viscosa | Verfahren zur Herstellung von lichtbeständigen Polymeren |
| GB1251971A (enExample) † | 1968-05-14 | 1971-11-03 | ||
| US3579483A (en) * | 1969-04-15 | 1971-05-18 | Allied Chem | Epsilon-caprolactam continuous polymerization process |
| CH520170A (de) * | 1969-07-09 | 1972-03-15 | Inventa Ag | Verfahren zur Herstellung hochmolekularer Polyamide |
| DE2033265A1 (de) * | 1970-07-04 | 1972-02-03 | Bayer | Verfahren zur Polymerisation von Lactamen |
| US3840500A (en) * | 1970-08-05 | 1974-10-08 | Inventa Ag | Process for the preparation of high molecular weight polyamides |
| GB1442749A (en) * | 1972-12-18 | 1976-07-14 | Ici Ltd | Catalytic polymerisation of dodecanolactam |
| US4111869A (en) * | 1974-02-28 | 1978-09-05 | Ceskoslovenska Akademie Ved | Method for the polymerization of lactams |
| US4471081A (en) † | 1983-05-27 | 1984-09-11 | Allied Corporation | Continuous low moisture catalytic method for polymerization of caprolactam |
| US4490521A (en) * | 1983-10-11 | 1984-12-25 | The Standard Oil Company | Preparation of spinnable polyamide from dinitrile/diamine/water with metal salt of oxygenated phosphorus compound catalyst |
| US4701518A (en) * | 1986-05-08 | 1987-10-20 | Monsanto Company | Antimicrobial nylon prepared in water with zinc compound and phosphorus compound |
| US4749776A (en) * | 1986-11-03 | 1988-06-07 | The Standard Oil Company | Process for the manufacture of polyamide from dinitrile and diamine in contact with an ester of an oxygenated phosphorus compound catalyst and a strong base |
| DE4103210A1 (de) * | 1991-02-02 | 1992-08-06 | Huels Chemische Werke Ag | Verfahren zur herstellung eines thermoplastisch verarbeitbaren, aromatischen polyamids |
| US5298594A (en) * | 1992-09-18 | 1994-03-29 | Chinese Petrochemical Development Corp. | Preparation of nylon 6 with alkali metal hypophosphite catalyst and organic phosphite catalyst |
-
1995
- 1995-02-15 CA CA002181236A patent/CA2181236C/en not_active Expired - Fee Related
- 1995-02-15 JP JP52190695A patent/JP3504664B2/ja not_active Expired - Lifetime
- 1995-02-15 EP EP95911758A patent/EP0745106B2/en not_active Expired - Lifetime
- 1995-02-15 WO PCT/US1995/001950 patent/WO1995022577A1/en not_active Ceased
- 1995-02-15 DE DE69500807T patent/DE69500807T3/de not_active Expired - Lifetime
-
1997
- 1997-03-24 US US08/822,886 patent/US5929200A/en not_active Expired - Lifetime
Patent Citations (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US3384615A (en) * | 1966-05-16 | 1968-05-21 | Grace W R & Co | Stabilization of polyamides |
| US4237034A (en) * | 1973-05-14 | 1980-12-02 | Imperial Chemical Industries Limited | Polyamide compositions containing carboxylic acid metal salt and organophosphonic acid |
Cited By (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1997043236A1 (de) * | 1996-05-14 | 1997-11-20 | Rathor Ag | Verfahren zur bromierung natürlicher ungesättigter öle |
| WO1999061522A1 (en) * | 1998-05-29 | 1999-12-02 | Solutia Inc. | Nucleation of polyamides in the presence of hypophosphite |
| EP1036819A4 (en) * | 1998-08-24 | 2001-08-01 | Asahi Chemical Ind | POLYAMIDE RESIN COMPOSITION AND METHOD FOR THE PRODUCTION THEREOF |
| US7491763B2 (en) | 2002-07-10 | 2009-02-17 | Asahi Kasei Chemicals Corporation | Polyamide composition |
| WO2005000953A3 (de) * | 2003-06-27 | 2005-03-17 | Ems Chemie Ag | Polyamidformmasse, verfahren zur herstellung der polyamidformmasse und formteile herstellbar aus der polyamidformmasse |
| US10865288B2 (en) | 2014-05-30 | 2020-12-15 | Ascend Performance Materials Operations Llc | Low phosphorus low color polyamides |
| WO2015183385A1 (en) * | 2014-05-30 | 2015-12-03 | Ascend Performance Materials Operations Llc | Low phosphorus low color polyamides |
| WO2020132002A1 (en) * | 2018-12-18 | 2020-06-25 | Ascend Performance Materials Operations Llc | Antimicrobial nonwoven polyamides with zinc content |
| WO2020132006A1 (en) * | 2018-12-18 | 2020-06-25 | Ascend Performance Materials Operations Llc | Antimicrobial polymer compositions, fibers, and yarns |
| EP3714090A1 (en) * | 2018-12-18 | 2020-09-30 | Ascend Performance Materials Operations LLC | Antimicrobial nonwoven polyamides with zinc content |
| US11185071B2 (en) | 2018-12-18 | 2021-11-30 | Ascend Performance Materials Operations Llc | Anti-microbial polymer compositions, fibers, and yarns |
| US11758909B2 (en) | 2018-12-18 | 2023-09-19 | Ascend Performance Materials Operations Llc | Antimicrobial nonwoven polyamides with zinc content |
| US12041931B2 (en) | 2018-12-18 | 2024-07-23 | Ascend Performance Materials Operations Llc | Antimicrobial polymer compositions, fibers, and yarns |
| US12336539B2 (en) | 2018-12-18 | 2025-06-24 | Ascend Performance Materials Operations Llc | Antimicrobial nonwoven polyamides with zinc content |
Also Published As
| Publication number | Publication date |
|---|---|
| DE69500807T2 (de) | 1998-04-09 |
| US5929200A (en) | 1999-07-27 |
| DE69500807T3 (de) | 2005-09-15 |
| DE69500807D1 (de) | 1997-11-06 |
| JP3504664B2 (ja) | 2004-03-08 |
| CA2181236C (en) | 2007-10-30 |
| EP0745106B1 (en) | 1997-10-01 |
| EP0745106A1 (en) | 1996-12-04 |
| CA2181236A1 (en) | 1995-08-24 |
| EP0745106B2 (en) | 2004-12-29 |
| JPH09512839A (ja) | 1997-12-22 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US5929200A (en) | Polyamides having improved color and processibility and process for manufacturing | |
| EP0684966B1 (en) | Polyamides having improved color and processibility and process for manufacturing | |
| US5763561A (en) | Polyamide compositions having improved thermal stability | |
| CA2136177C (en) | Manufacture of terephthalic acid copolyamides | |
| US5663284A (en) | Copolymerized polyamide and a production process/thereof | |
| US20110190442A1 (en) | Nylon resins and process | |
| US4237034A (en) | Polyamide compositions containing carboxylic acid metal salt and organophosphonic acid | |
| EP0655076B1 (en) | High pressure process for the manufacture of terephthalic acid copolyamides | |
| JPS5946974B2 (ja) | 透明な高分子コポリアミド | |
| US5191060A (en) | Preparation of dodecane terephthalamide polymers | |
| JP2016521795A (ja) | 固相重合を含む脂肪族または部分芳香族のポリアミドの製造法 | |
| US5298597A (en) | Aqueous preparation of polyamide with catalyst mixture | |
| US5502155A (en) | Manufacture of partially aromatic polyamides | |
| CA2229461C (en) | Process for the manufacture of nylon compositions with improved flow | |
| US4587309A (en) | Process for producing polyetheresteramides | |
| US5298594A (en) | Preparation of nylon 6 with alkali metal hypophosphite catalyst and organic phosphite catalyst | |
| US5298598A (en) | Preparation of polyamide with mixture of phosphorus catalysts | |
| US5290747A (en) | Nylon 6 catalyst system | |
| US3431236A (en) | Method of adding an antioxidant to a continuous polymerization process | |
| JPH07238222A (ja) | 熱黄変性の改善されたポリアミド組成物 | |
| JPH01104653A (ja) | ポリアミドの製造方法 | |
| JPH06192569A (ja) | 難燃性の熱可塑性ポリアミド | |
| US5264406A (en) | Catalyst system for polyamide and copolyamide | |
| KR101557540B1 (ko) | 공중합 폴리아미드 수지, 이의 제조방법 및 이를 포함하는 성형품 | |
| EP0445810A2 (en) | Polyamide monofilament |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): CA JP |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 2181236 Country of ref document: CA |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1995911758 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1995911758 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1995911758 Country of ref document: EP |