US20020001725A1 - Low refractive index sio2 film and process for producing the same - Google Patents

Low refractive index sio2 film and process for producing the same Download PDF

Info

Publication number
US20020001725A1
US20020001725A1 US08/985,904 US98590497A US2002001725A1 US 20020001725 A1 US20020001725 A1 US 20020001725A1 US 98590497 A US98590497 A US 98590497A US 2002001725 A1 US2002001725 A1 US 2002001725A1
Authority
US
United States
Prior art keywords
film
refractive index
sio
low refractive
alkyl group
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Abandoned
Application number
US08/985,904
Other languages
English (en)
Inventor
Koji Ichimura
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dai Nippon Printing Co Ltd
Original Assignee
Dai Nippon Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dai Nippon Printing Co Ltd filed Critical Dai Nippon Printing Co Ltd
Assigned to DAI NIPPON PRINTING CO., LTD. reassignment DAI NIPPON PRINTING CO., LTD. ASSIGNMENT OF ASSIGNORS INTEREST (SEE DOCUMENT FOR DETAILS). Assignors: ICHIMURA, KOJI
Publication of US20020001725A1 publication Critical patent/US20020001725A1/en
Priority to US10/470,580 priority Critical patent/US7348041B2/en
Abandoned legal-status Critical Current

Links

Images

Classifications

    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/11—Anti-reflection coatings
    • G02B1/111—Anti-reflection coatings using layers comprising organic materials
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/40—Oxides
    • C23C16/401—Oxides containing silicon
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00—Stock material or miscellaneous articles
    • Y10T428/31504—Composite [nonstructural laminate]
    • Y10T428/31652—Of asbestos
    • Y10T428/31663—As siloxane, silicone or silane
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00—Stock material or miscellaneous articles
    • Y10T428/31504—Composite [nonstructural laminate]
    • Y10T428/31652—Of asbestos
    • Y10T428/31667—Next to addition polymer from unsaturated monomers, or aldehyde or ketone condensation product

Definitions

  • the present invention relates to a low refractive index SiO 2 film which is applicable to a light antireflection film on various surfaces of curve mirrors, back mirrors, goggles, window glasses, displays of personal computers and word processors, and other various commercial displays.
  • antireflection films have been applied to surfaces of various displays of word processors, computers, and televisions, surfaces of various optical lenses and optical articles, and surfaces of window glasses of automobiles and electric railcars to prevent the reflection of light from the above surfaces.
  • n 0 ⁇ square root ⁇ square root over ( n g ) ⁇ (1)
  • ⁇ 0 represents a specific wavelength
  • n 0 represents the refractive index of the antireflection film at this wavelength
  • h represents the thickness of the antireflection film
  • n g represents the refractive index of the substrate.
  • the refractive index n g of glass is about 1.5
  • the refractive index no of MgF 2 film is 1.38
  • the wavelength ⁇ 0 of incident light is 5500 ⁇ (reference).
  • the results of calculation show that the thickness h of the antireflection film is about 0.1 ⁇ m which is the thickness of an optical thin film.
  • an optical thin film having such thickness has been used as the antireflection film.
  • Vacuum process such as vacuum deposition, sputtering, ion plating, and plasma CVD, have been known to be suitable for the formation of such an optical thin film.
  • An SiO 2 film is generally known as a low refractive index film and hence has been extensively used as antireflection films and the like.
  • Antireflection films having various layer constructions, however, have been desired to have lower refractive index.
  • an object of the present invention is to provide a low refractive index SiO 2 film which uses a starting material for forming an SiO 2 film and has a lower refractive index than the conventional SiO 2 film.
  • a low refractive index SiO 2 film comprising an SiO 2 film with a low refractive index element introduced thereinto, the low refractive index element being at least one member selected from the group consisting of a fluorine atom, an alkyl group having 1 to 4 carbon atoms, and an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom.
  • Formation of a film in such a state that at least one low refractive index element selected from the group consisting of a fluorine atom, an alkyl group having 1 to 4 carbon atoms, and an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom is introduced into an SiO 2 -forming material, can provide a film having a lower refractive index than the SiO 2 film per se.
  • the SiO 2 film with an low refractive index element introduced thereinto according to the present invention has lower refractive index than the SiO 2 film per se and hence is useful as a film as the upper layer in an antireflection film.
  • An SiO 2 film with a fluorine atom introduced thereinto is usually in such a state that a silicon atom is bonded to a fluorine atom.
  • the bond is likely to be hydrolyzed by moisture in air, causing the low refractive index effect to be lost. Therefore, according to a preferred embodiment of the present invention, an alkyl group with a part or the whole of hydrogen atoms substituted by a fluorine atom is used as the starting material.
  • the fluorine atom introduced into the SiO 2 film is bonded to the carbon atom, causing no hydrolysis, which permits the low refractive index effect to be maintained for a long period of time.
  • a process for producing a low refractive index SiO 2 film comprising forming a thin film on a substrate by CVD using a starting material gas comprising a gas containing a fluorine atom, a gas containing a silicon atom and an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom, and a gas containing an oxygen atom.
  • a mixed gas comprising a gas containing a fluorine atom, a volatile gas of an organic compound containing a silicon atom and an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom, and a gas containing an oxygen atom, into a vacuum chamber maintained in a vacuum of 10 ⁇ 3 to 1 mmHg (Torr) and bringing the mixed gas to a plasma stream by glow discharge; and
  • the resultant CVD film comprises a substantially inorganic SiO 2 film formed by oxidation of Si atom and, introduced into the SiO 2 film, a fluorine atom and/or an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom, that is, a low refractive index element.
  • the SiO 2 film with a low refractive index element introduced thereinto has a lower refractive index than an SiO 2 film not using a gas containing a low refractive index element, that is, an SiO 2 film per se. Further, the low refractive index film has high hardness and bond strength.
  • FIG. 1 is a schematic diagram showing an embodiment of the construction of a plasma CVD apparatus for producing the low refractive index SiO 2 film according to the present invention.
  • FIG. 1 A schematic diagram showing an embodiment of the construction of a plasma CVD apparatus for producing the low refractive index SiO 2 film according to the present invention is shown in FIG. 1.
  • numeral 1 designates a vacuum chamber the interior of which can be regulated to a desired degree of vacuum.
  • a winding/unwinding mechanism containing a pair of rolls 3 , 4 which can unwind or rewind a web 2 and function to travel the web 2 in a positive direction or in a reverse direction, is disposed within the vacuum chamber 1 .
  • a plasma zone 5 is disposed so as to face the surface of the web 2 travelled between the roll 3 and the roll 4 .
  • the plasma zone 5 for plasma CVD treatment comprises a section for projecting a mixed starting material gas, a flat electrode 6 , and a film forming drum 7 which can stably travel the web 2 and is grounded.
  • the flat electrode 6 may be a gas projecting electrode which projects an inert gas to create plasma.
  • a gas containing a fluorine atom, a gas containing a silicon atom and an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom, and a gas containing an oxygen atom are used as the starting material for forming a low refractive index SiO 2 film by CVD according to the present invention.
  • the gas containing a fluorine atom is added in order to make the refractive index of the resultant film lower than that of the SiO 2 film per se, and examples thereof include CF 4 , C 2 F 6 , C 3 F 6 , and SF 6 .
  • the material containing a silicon atom and an alkyl group having 1 to 4 carbon atoms is a main starting material for the low refractive index film.
  • the alkyl group having 1 to 4 carbon atoms, particularly a methyl or ethyl group, is introduced in order to make the refractive index of the resultant film lower than that of the SiO 2 film per se.
  • the starting material containing a silicon atom and an alkyl group having 1 to 4 carbon atoms is gasified upon introduction into the vacuum chamber.
  • the reason why the number of carbon atoms of the alkyl group in the material to be gasified is limited to 1 to 4 is that a starting material containing an alkyl group having 5 or more carbon atoms is less likely to be vaporized in CVD, making it difficult to form a low refractive index film.
  • Gasifiable starting materials containing a silicon atom and an alkyl group having 1 to 4 carbon atoms include silicon-containing organic compounds, such as hexamethyldisiloxane (abbreviation: HMDSO), tetramethyldisiloxane (abbreviation: TMDSO), octamethylcyclotetrasiloxane, tetraethoxysilane (abbreviation: TEOS), methyltrimethoxysilane (abbreviation: MTMOS), methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, and phenylsilane.
  • HMDSO hexamethyldisiloxane
  • TMDSO tetramethyldisiloxane
  • TEOS tetraethoxysilane
  • MTMOS methyltrimethoxysilane
  • HMDSO is particularly preferred.
  • the molecule contains an alkyl group having 1 to 4 carbon atoms, such as a methyl or ethyl group, a silicon atom, and an oxygen atom.
  • the material containing a silicon atom and an alkyl group having 1 to 4 carbon atoms as the main starting material is such that a part or the whole of hydrogen atoms in the alkyl group having 1 to 4 carbon atoms has been substituted by a fluorine atom.
  • the fluorine atom is stably bonded to the carbon atom to offer the effect of stably maintaining the low refractive index effect.
  • Gasifiable starting materials containing a silicon atom and an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms substituted by a fluorine atom
  • gasifiable starting materials include HMDSO, TMDSO, octamethylcyclotetrasiloxane, TEOS, MTMOS, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, and phenylsilane, a part or the whole of hydrogen atoms in each of the above compounds being substituted by a fluorine atom.
  • the gas containing an oxygen atom is used in order to oxidize the Si material to give SiO 2 .
  • gaseous materials may be added to the mixed gas composed of the above gases from the viewpoint of imparting desired properties.
  • the flow (SLM) ratio is preferably 1:0.1 to 20.
  • the vacuum chamber is preferably kept at a pressure of 10 ⁇ 3 to 1 mmHg (Torr).
  • An antireflection film will be described as a preferred example of products with the low refractive index SiO 2 film, according to the present invention, formed thereon.
  • a polyethylene terephthalate (PET) substrate (a product of Toray Industries, Inc., tradename: Lumirror T-60, thickness: 100 ⁇ m) is provided as a substrate.
  • PET polyethylene terephthalate
  • a 125 ⁇ -thick ITO layer, a 250 ⁇ -thick SiO 2 layer, a 1000 ⁇ -thick ITO layer, and a 800 ⁇ -thick SiO 2 layer are laminated in that order on the PET substrate.
  • the ITO layer may be formed by any means. In general, however, sputtering is applicable.
  • a TiO 2 or other layer formed of a high refractive index material may be used instead of the ITO layer.
  • the higher the degree to which the refractive index of the layer underlying the SiO 2 layer is above the refractive index of the SiO 2 layer the better the antireflection effect and consequently the better the performance of the antireflection film.
  • electrical conductivity can be imparted to the film, permitting the film to exhibit an electromagnetic shielding property and an antistatic property.
  • a fluororesin layer having a thickness of not more than 100 ⁇ may be wet coated thereon from the viewpoint of forming an antismudge coating which functions to enhance the water repellency of the surface, thereby preventing the adhesion of a stain such as a fingerprint.
  • the ITO layer and the SiO 2 layer which are first formed on the hard coat layer on the substrate, may be replaced with a wet coat of an organic material.
  • Formation of the ITO layer by sputtering takes a lot of time which is causative of increased production cost.
  • Such a change in film forming means is advantageous from the viewpoint of the cost.
  • the adhesion of the ITO layer formed on the wet coat layer of the organic material is not very good. In this case, a layer having a small thickness (usually not more than 100 ⁇ ) of other material corresponding to an adhesive may be formed between the organic layer and the ITO layer.
  • an SiO 2 layer alone may be formed on the hard coat.
  • This layer construction is extensively adopted in the antireflection film for LCD from the viewpoint of the cost.
  • TAC a product of Fuji Photo Film Co., Ltd., tradename: Fuji Tac, thickness: 100 ⁇ m
  • possessing optical properties, that is, not having birefringence may be used as the substrate.
  • TMDSO, oxygen, and CF 4 were used as starting material gases, and argon was used as a gas for producing plasma. These gases were introduced, as a mixed gas composed of TMDSO (0.1 SLM), oxygen (20 SLM), CF 4 (0.22 SLM), and argon (0.35 SLM), into a vacuum chamber of a plasma CVD apparatus with a pressure regulated to 40 mTorr (4 ⁇ 10 ⁇ 2 mmHg), and an electric power of 2.1 kW and 40 kHz was applied between the film forming drum and the gas projecting electrode to produce plasma.
  • a PET film (a product of Toray Industries, Inc., Japan; tradename: Lumirror T-60, thickness: 100 ⁇ m) as a substrate was fed into and passed through a plasma producing zone at a feed rate of 1.5 m/min to form an SiO 2 film on the substrate.
  • the antireflection effect of the SiO 2 film was confirmed as follows. A black vinyl tape was applied to the back surface of the substrate to eliminate the reflection of the back surface. In this state, the reflectance of the front surface in the visible light region was measured at an incident angle of 5°, and the refractive index of the SiO 2 film was evaluated based on the minimum reflectance. As a result, it was found that the minimum reflectance was 1.76% and the refractive index was 1.47.
  • the SiO 2 film formed without use of CF 4 had a minimum reflectance of 1.95% and a refractive index of 1.483.
  • the SiO 2 film formed using CF 4 in Example 1 had lower reflectance and lower refractive index.
  • Oxygen was used as a part of the starting material, and argon was used as a carrier gas for producing plasma. These gases were introduced, as a mixed gas composed of oxygen (30 sccm) and argon (30 sccm), into a vacuum chamber of a plasma CVD apparatus with a pressure regulated to 40 mTorr. HMDSO (hexamethyldisiloxane) as a monomer material was bubbled by this carrier gas to feed the monomer material into the vacuum chamber of the CVD apparatus with a pressure regulated to 40 mTorr. The bubbling temperature was room temperature. Plasma was produced by applying an electric power of 100 W and 13.56 MHz across the upper electrode and the earth electrode.
  • HMDSO hexamethyldisiloxane
  • a PET film [a product of Toray Industries, Inc., tradename: Lumirror T-60, thickness: 100 ⁇ m] was used as a substrate, and the film formation time was 10 min.
  • the refractive index of the film thus formed was measured by ellipsometry and found to be 1.42.
  • the film was analyzed by IR spectrometry for the presence of a CH 3 group. As a result, a peak derived from stretching of an Si—CH 3 bond appeared around 1277 cm ⁇ 1, indicating the presence of the CH 3 group.
  • Example 2 For comparison, the procedure of Example 2 was repeated, except that the flow rate of oxygen was 100 sccm. Thus, an SiO 2 film of Comparative Example 2 was formed. The SiO 2 film was analyzed by IR spectroscopy. As a result, the presence of a CH 3 group was hardly observed. The refractive index of the SiO 2 film formed in Comparative Example 2 was measured by ellipsometry and found to be 1.44, which was higher than the refractive index of the SiO 2 film, with the CH 3 group introduced thereinto, prepared in Example 2.
  • a PET film (a product of Toray Industries, Inc., tradename: Lumirror T-60, thickness: 100 ⁇ m) was provided as a substrate.
  • Oxygen, argon, and CF 4 were used as the starting material gases.
  • HMDSO hexamethyldisiloxane
  • the gas flow rate was 30 sccm for oxygen, 30 sccm for argon, and 30 sccm for CF 4 .
  • the monomer material was bubbled using the argon gas as a carrier gas and fed into a vacuum chamber of a plasma CVD apparatus with the pressure being regulated to 40 mTorr. The bubbling temperature was room temperature.
  • a PET film (a product of Toray Industries, Inc., tradename: Lumirror T-60, thickness: 100 ⁇ m) was provided as a substrate.
  • Oxygen and argon were used as the starting material gases.
  • HMDSO hexamethyldisiloxane
  • the gas flow rate was 30 sccm for oxygen and 30 sccm for argon.
  • the monomer material was bubbled using the argon gas as a carrier gas and fed into a vacuum chamber of a plasma CVD apparatus with the pressure being regulated to 40 mTorr. The bubbling temperature was room temperature.
  • the refractive index SiO 2 film with at least one low refractive index element selected from a fluorine atom, an alkyl group having 1 to 4 carbon atoms, and an alkyl group having 1 to 4 carbon atoms with a part or the whole of hydrogen atoms thereof being substituted by a fluorine atom has lower refractive index than the SiO 2 film with no low refractive index element introduced thereinto.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Physics & Mathematics (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Mechanical Engineering (AREA)
  • Metallurgy (AREA)
  • General Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Physics & Mathematics (AREA)
  • Optics & Photonics (AREA)
  • Chemical Vapour Deposition (AREA)
  • Surface Treatment Of Optical Elements (AREA)
  • Laminated Bodies (AREA)
  • Surface Treatment Of Glass (AREA)
US08/985,904 1996-12-18 1997-12-05 Low refractive index sio2 film and process for producing the same Abandoned US20020001725A1 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
US10/470,580 US7348041B2 (en) 1996-12-18 2003-04-09 Antireflection film made of a CVD SiO2 film containing a fluoro and/or alkyl modifier

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP354141/1996 1996-12-18
JP35414196 1996-12-18
JP31599297A JP3773340B2 (ja) 1996-12-18 1997-10-31 低屈折率SiO2 膜及びその製造方法
JP315992/1997 1997-10-31

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US10/470,580 Continuation US7348041B2 (en) 1996-12-18 2003-04-09 Antireflection film made of a CVD SiO2 film containing a fluoro and/or alkyl modifier

Publications (1)

Publication Number Publication Date
US20020001725A1 true US20020001725A1 (en) 2002-01-03

Family

ID=26568491

Family Applications (2)

Application Number Title Priority Date Filing Date
US08/985,904 Abandoned US20020001725A1 (en) 1996-12-18 1997-12-05 Low refractive index sio2 film and process for producing the same
US10/470,580 Expired - Fee Related US7348041B2 (en) 1996-12-18 2003-04-09 Antireflection film made of a CVD SiO2 film containing a fluoro and/or alkyl modifier

Family Applications After (1)

Application Number Title Priority Date Filing Date
US10/470,580 Expired - Fee Related US7348041B2 (en) 1996-12-18 2003-04-09 Antireflection film made of a CVD SiO2 film containing a fluoro and/or alkyl modifier

Country Status (4)

Country Link
US (2) US20020001725A1 (enExample)
EP (1) EP0849374B1 (enExample)
JP (1) JP3773340B2 (enExample)
DE (1) DE69729429T2 (enExample)

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US10221486B2 (en) * 2013-09-27 2019-03-05 Sumitomo Chemical Company, Limited Laminate film, organic electroluminescence device, photoelectric conversion device, and liquid crystal display
EP3693766A1 (en) * 2019-02-05 2020-08-12 Corporation de L'Ecole Polytechnique de Montreal Article coated with a low refractive index layer based on fluorinated organosilicon compounds
EP3693765A1 (en) * 2019-02-05 2020-08-12 Essilor International (Compagnie Generale D'optique) Article coated with an antireflective coating having improved optical properties
US20220235240A1 (en) * 2019-07-26 2022-07-28 Jiangsu Favored Nanotechnology Co., Ltd. Water-resistant nanofilm, preparation method and article thereof

Families Citing this family (15)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6627532B1 (en) 1998-02-11 2003-09-30 Applied Materials, Inc. Method of decreasing the K value in SiOC layer deposited by chemical vapor deposition
US6054379A (en) 1998-02-11 2000-04-25 Applied Materials, Inc. Method of depositing a low k dielectric with organo silane
US6340435B1 (en) 1998-02-11 2002-01-22 Applied Materials, Inc. Integrated low K dielectrics and etch stops
US6593247B1 (en) 1998-02-11 2003-07-15 Applied Materials, Inc. Method of depositing low k films using an oxidizing plasma
JP2000121804A (ja) * 1998-10-09 2000-04-28 Sekisui Chem Co Ltd 反射防止フィルム
JP2002103507A (ja) * 2000-09-29 2002-04-09 Dainippon Printing Co Ltd シリカ層、及びシリカ層を用いた反射防止フィルム
DE102005007825B4 (de) 2005-01-10 2015-09-17 Interpane Entwicklungs-Und Beratungsgesellschaft Mbh Verfahren zur Herstellung einer reflexionsmindernden Beschichtung, reflexionsmindernde Schicht auf einem transparenten Substrat sowie Verwendung einer derartigen Schicht
JP4807195B2 (ja) * 2006-09-08 2011-11-02 旭硝子株式会社 低屈折率膜の製膜方法および低屈折率膜を有する物品
CN101631661B (zh) * 2007-06-25 2012-03-14 夏普株式会社 烧制装置
US20090274930A1 (en) * 2008-04-30 2009-11-05 Guardian Industries Corp. Alkaline earth fluoride coatings deposited via combustion deposition
FR2985255B1 (fr) * 2011-12-28 2015-08-07 Ecole Polytech Article revetu d'un revetement interferentiel ayant des proprietes stables dans le temps.
US9025100B2 (en) 2012-11-30 2015-05-05 Apple Inc. Display with shielding antireflection layer
FR3007024A1 (fr) * 2013-06-14 2014-12-19 Essilor Int Article revetu d'une couche de nature silico-organique ameliorant les performances d'un revetement externe
JP2024146003A (ja) * 2023-03-31 2024-10-15 ホヤ レンズ タイランド リミテッド 眼鏡レンズ及び眼鏡
CN122663517A (zh) 2023-12-19 2026-08-28 依视路国际公司 包括对透射和反射两者提供调制的电致变色叠层的光学制品

Family Cites Families (16)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4419386A (en) * 1981-09-14 1983-12-06 Gordon Roy G Non-iridescent glass structures
US5759643A (en) 1987-01-16 1998-06-02 Seiko Epson Corporation Polarizing plate and method of production
US5264286A (en) * 1988-03-03 1993-11-23 Asahi Glass Company Ltd. Laminated glass structure
CA2054094C (en) 1990-10-25 1999-12-21 Kazufumi Ogawa Chemically adsorbed monomolecular lamination film
EP0584252B1 (en) * 1991-05-17 1998-03-04 Lam Research Corporation A PROCESS FOR DEPOSITING A SIOx FILM HAVING REDUCED INTRINSIC STRESS AND/OR REDUCED HYDROGEN CONTENT
JP2699695B2 (ja) * 1991-06-07 1998-01-19 日本電気株式会社 化学気相成長法
DE69331291T2 (de) * 1992-11-13 2002-08-08 Energy Conversion Devices, Inc. Verfahren zur Herstellung einer Sperrbeschichtung mittels plasmaunterstütztem CVD
US5364666A (en) * 1993-09-23 1994-11-15 Becton, Dickinson And Company Process for barrier coating of plastic objects
JPH0790589A (ja) * 1993-09-24 1995-04-04 G T C:Kk シリコン酸化膜の形成方法
US5909314A (en) * 1994-02-15 1999-06-01 Dai Nippon Printing Co., Ltd. Optical functional materials and process for producing the same
US5563105A (en) * 1994-09-30 1996-10-08 International Business Machines Corporation PECVD method of depositing fluorine doped oxide using a fluorine precursor containing a glass-forming element
EP0724286A1 (en) * 1995-01-25 1996-07-31 Applied Materials, Inc. A method of forming a thin film of silicon oxide for a semiconductor device
US5571576A (en) * 1995-02-10 1996-11-05 Watkins-Johnson Method of forming a fluorinated silicon oxide layer using plasma chemical vapor deposition
JPH09203817A (ja) * 1996-01-26 1997-08-05 Toyo Commun Equip Co Ltd 光導波路カプラ
SG53005A1 (en) 1996-07-03 1998-09-28 Novellus Systems Inc Method for depositing substituted fluorcarbon polymeric layers
DE19650784A1 (de) 1996-12-06 1998-06-10 Bosch Gmbh Robert Vorrichtung für eine Kraftstoffversorgungsanlage

Cited By (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US10221486B2 (en) * 2013-09-27 2019-03-05 Sumitomo Chemical Company, Limited Laminate film, organic electroluminescence device, photoelectric conversion device, and liquid crystal display
EP3693766A1 (en) * 2019-02-05 2020-08-12 Corporation de L'Ecole Polytechnique de Montreal Article coated with a low refractive index layer based on fluorinated organosilicon compounds
EP3693765A1 (en) * 2019-02-05 2020-08-12 Essilor International (Compagnie Generale D'optique) Article coated with an antireflective coating having improved optical properties
WO2020161128A1 (en) * 2019-02-05 2020-08-13 Corporation De L'ecole Polytechnique De Montreal Article coated with a low refractive index layer based on fluorinated organosilicon compounds
WO2020161141A1 (en) * 2019-02-05 2020-08-13 Essilor International Article coated with an antireflective coating having improved optical properties
CN113396344A (zh) * 2019-02-05 2021-09-14 依视路国际公司 涂覆有减反射涂层的具有改善的光学特性的制品
CN113439222A (zh) * 2019-02-05 2021-09-24 蒙特利尔综合理工学院公司 涂覆有基于氟化有机硅化合物的低折射率层的制品
US12117591B2 (en) 2019-02-05 2024-10-15 Corporation De L'ecole Polytechnique De Montreal Article coated with a low refractive index layer based on fluorinated organosilicon compounds
US12210136B2 (en) 2019-02-05 2025-01-28 Essilor International Article coated with an antireflective coating having improved optical properties
US20220235240A1 (en) * 2019-07-26 2022-07-28 Jiangsu Favored Nanotechnology Co., Ltd. Water-resistant nanofilm, preparation method and article thereof
US12173175B2 (en) * 2019-07-26 2024-12-24 Jiangsu Favored Nanotechnology Co., Ltd. Water-resistant nanofilm, preparation method and article thereof

Also Published As

Publication number Publication date
EP0849374A3 (en) 1999-06-30
EP0849374A2 (en) 1998-06-24
JP3773340B2 (ja) 2006-05-10
DE69729429T2 (de) 2005-06-16
EP0849374B1 (en) 2004-06-09
DE69729429D1 (de) 2004-07-15
JPH10230561A (ja) 1998-09-02
US7348041B2 (en) 2008-03-25
US20040157061A1 (en) 2004-08-12

Similar Documents

Publication Publication Date Title
US7348041B2 (en) Antireflection film made of a CVD SiO2 film containing a fluoro and/or alkyl modifier
JP4908661B2 (ja) 反射防止膜
CA1329567C (en) Coated article and method of manufacturing the article
CN103958731B (zh) 通过常压化学气相沉积沉积氧化硅
JPH04251736A (ja) 薄いガスバリヤーフィルム及びその迅速な蒸着方法
JP2005096322A (ja) 機能性層転写フィルム、並びに、防汚層及び機能性層転写体
US20040018362A1 (en) Silica layers and antireflection film using same
JP3679074B2 (ja) 透明積層フィルム、偏光板、液晶表示素子及び液晶表示装置
JP2005017544A (ja) 反射防止フィルム、および画像表示装置
Kakiuchi et al. Silicon oxide coatings with very high rates (> 10 nm/s) by hexamethyldisiloxane-oxygen fed atmospheric-pressure VHF plasma: film-forming behavior using cylindrical rotary electrode
US20040121167A1 (en) Process for depositing finely dispersed organic-inorganic films and articles made therefrom
JP2004258394A (ja) 光学機能性膜、反射防止フィルム、偏光板および表示装置
JP3699877B2 (ja) 積層フィルムの製造方法
JPH11256339A (ja) 撥水性コーティング膜、防汚性物品、及び撥水性コーティング膜の製造方法
JP4014357B2 (ja) 撥水性防汚フィルム
JP2006071982A (ja) 紫外線吸収反射防止フィルム、および画像表示装置
JP3751922B2 (ja) 反射防止フィルム、およびこれを用いたディスプレイ装置、液晶ディスプレイ装置
JP4278162B2 (ja) 反射防止フィルム
JP3732451B2 (ja) 透明積層フィルムの製造方法及び透明積層フィルム及び反射防止フィルム
JP2004255635A (ja) 透明積層フィルム、反射防止フィルム及びそれを用いた偏光板、液晶表示装置
JP2000338307A (ja) 反射防止フィルム
JP2004223769A (ja) 透明積層フィルム、反射防止フィルム及びそれを用いた偏光板、液晶表示装置
JPH04366901A (ja) 炭素膜を有する素子
JP2014168934A (ja) ガスバリア性フィルムおよびガスバリア性フィルムの製造方法
JP2005055724A (ja) 反射防止フィルム、および画像表示装置

Legal Events

Date Code Title Description
AS Assignment

Owner name: DAI NIPPON PRINTING CO., LTD., JAPAN

Free format text: ASSIGNMENT OF ASSIGNORS INTEREST;ASSIGNOR:ICHIMURA, KOJI;REEL/FRAME:009033/0542

Effective date: 19980129

STCB Information on status: application discontinuation