JPH10245497A - 黒色顔料 - Google Patents
黒色顔料Info
- Publication number
- JPH10245497A JPH10245497A JP8717297A JP8717297A JPH10245497A JP H10245497 A JPH10245497 A JP H10245497A JP 8717297 A JP8717297 A JP 8717297A JP 8717297 A JP8717297 A JP 8717297A JP H10245497 A JPH10245497 A JP H10245497A
- Authority
- JP
- Japan
- Prior art keywords
- aniline
- black
- salt
- black pigment
- acid
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】
【課題】 クロム塩や銅塩を製造時に使わなくてもよく
て且つ製品中にも含まない、アニリンの酸化縮合物であ
るアニリンブラックの製造方法。 【解決手段】 塩酸や硫酸などの酸により可溶性にした
アニリン水溶液中へ、例えば鉄、ニッケル等の金属又は
それらの化合物を単独又は混合物として存在させ、そこ
へ過酸化水素を注加することによって得られる。
て且つ製品中にも含まない、アニリンの酸化縮合物であ
るアニリンブラックの製造方法。 【解決手段】 塩酸や硫酸などの酸により可溶性にした
アニリン水溶液中へ、例えば鉄、ニッケル等の金属又は
それらの化合物を単独又は混合物として存在させ、そこ
へ過酸化水素を注加することによって得られる。
Description
【0001】
【発明の属する技術分野】本発明は、絵画用絵具、ポス
ターカラー、樹脂練り込み着色用、その他の着色を目的
とする分野で使用されるアニリンブラックの製造方法に
関する。
ターカラー、樹脂練り込み着色用、その他の着色を目的
とする分野で使用されるアニリンブラックの製造方法に
関する。
【0002】
【従来の技術】上記技術分野において、従来より使用さ
れているアニリンブラック中には、製造時に酸化剤や触
媒として使用されたクロム塩及び銅塩が、残留物として
多量に含まれている。
れているアニリンブラック中には、製造時に酸化剤や触
媒として使用されたクロム塩及び銅塩が、残留物として
多量に含まれている。
【0003】
【発明が解決しようとする課題】マット性のある黒色顔
料が他に無いために、環境や体に有害なクロム塩や銅塩
を多量に含んだアニリンブラックが現在使用され続けて
いる。従って、環境や体に有害なクロム塩や銅塩を、製
造時に使わなくてもよくて且つ製品中にも含まないアニ
リンブラックの製造方法が求められている。
料が他に無いために、環境や体に有害なクロム塩や銅塩
を多量に含んだアニリンブラックが現在使用され続けて
いる。従って、環境や体に有害なクロム塩や銅塩を、製
造時に使わなくてもよくて且つ製品中にも含まないアニ
リンブラックの製造方法が求められている。
【0004】
【課題を解決するための手段】上記課題は以下の本発明
によって達成される。塩酸や硫酸などの酸により可溶性
にしたアニリン水溶液中に、例えば鉄、ニッケル、銀、
金、白金等の金属又はそれらの化合物を単独又は混合物
として存在させ、そこへの過酸化水素の添加によりOH
ラジカルを発生させ、そのOHラジカルを酸化剤として
作用させることにより、アニリンは酸化縮合されてアニ
リンブラックが得られる。
によって達成される。塩酸や硫酸などの酸により可溶性
にしたアニリン水溶液中に、例えば鉄、ニッケル、銀、
金、白金等の金属又はそれらの化合物を単独又は混合物
として存在させ、そこへの過酸化水素の添加によりOH
ラジカルを発生させ、そのOHラジカルを酸化剤として
作用させることにより、アニリンは酸化縮合されてアニ
リンブラックが得られる。
【0005】
実施例1 62%硫酸3.0gと35%塩酸5.3gと水50ml
に、アニリン5.0gを入れ、攪拌溶解した後そこへ硫
酸第一鉄2.2gを水10mlに溶解したものを添加す
る。液温10〜15℃にて攪拌混合しながら、有効濃度
30%の過酸化水素15.0gを4時間にて注加し、そ
の後4時間攪拌混合を行い反応終了とする。反応終了
後、反応液を濾過水洗しペースト状黒色結晶を得る。こ
のペースト状黒色結晶を160mlの水を用いスラリー
とし、カセイソーダにてPH7.0に中和した後濾過乾
燥すると、アニリンブラック4.3gを得る。
に、アニリン5.0gを入れ、攪拌溶解した後そこへ硫
酸第一鉄2.2gを水10mlに溶解したものを添加す
る。液温10〜15℃にて攪拌混合しながら、有効濃度
30%の過酸化水素15.0gを4時間にて注加し、そ
の後4時間攪拌混合を行い反応終了とする。反応終了
後、反応液を濾過水洗しペースト状黒色結晶を得る。こ
のペースト状黒色結晶を160mlの水を用いスラリー
とし、カセイソーダにてPH7.0に中和した後濾過乾
燥すると、アニリンブラック4.3gを得る。
【0006】実施例2 62%硫酸6.2gと水65mlに、アニリン5.0g
を入れ、攪拌溶解した後そこへ塩化第二鉄3.6gを水
15mlに溶解したものを添加する。液温10℃にて攪
拌混合しながら、有効濃度30%の過酸化水素15.0
gを4時間にて注加し、その後4時間攪拌混合を行い反
応終了とする。反応終了後、反応液を濾過水洗しペース
ト状黒色結晶を得る。このペースト状黒色結晶を160
mlの水を用いスラリーとし、カセイソーダにてPH
7.0に中和した後濾過乾燥すると、アニリンブラック
4.5gを得る。
を入れ、攪拌溶解した後そこへ塩化第二鉄3.6gを水
15mlに溶解したものを添加する。液温10℃にて攪
拌混合しながら、有効濃度30%の過酸化水素15.0
gを4時間にて注加し、その後4時間攪拌混合を行い反
応終了とする。反応終了後、反応液を濾過水洗しペース
ト状黒色結晶を得る。このペースト状黒色結晶を160
mlの水を用いスラリーとし、カセイソーダにてPH
7.0に中和した後濾過乾燥すると、アニリンブラック
4.5gを得る。
Claims (1)
- 【請求項1】 過酸化水素と、それの分解触媒となりう
る金属又は金属塩を用い、発生するOHラジカルを酸化
剤としてアニリンを酸化させてなる、アニリンの酸化縮
合物であるアニリンブラックの製造方法。