CN107269023A CN201710721872.0A CN201710721872A CN107269023A CN 107269023 A CN107269023 A CN 107269023A CN 201710721872 A CN201710721872 A CN 201710721872A CN 107269023 A CN107269023 A CN 107269023A
Authority
CN
China
Prior art keywords
floor
reinforcing steel
presstressed reinforcing
reinforcement
concrete
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710721872.0A
Other languages
English (en)
Inventor
叶香雄
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201710721872.0A priority Critical patent/CN107269023A/zh
Publication of CN107269023A publication Critical patent/CN107269023A/zh
Pending legal-status Critical Current

Links

Classifications

    • EFIXED CONSTRUCTIONS
    • E04BUILDING
    • E04GSCAFFOLDING; FORMS; SHUTTERING; BUILDING IMPLEMENTS OR AIDS, OR THEIR USE; HANDLING BUILDING MATERIALS ON THE SITE; REPAIRING, BREAKING-UP OR OTHER WORK ON EXISTING BUILDINGS
    • E04G23/00Working measures on existing buildings
    • E04G23/02Repairing, e.g. filling cracks; Restoring; Altering; Enlarging
    • E04G23/0218Increasing or restoring the load-bearing capacity of building construction elements
    • E04G23/0237Increasing or restoring the load-bearing capacity of building construction elements of storey floors
    • EFIXED CONSTRUCTIONS
    • E04BUILDING
    • E04GSCAFFOLDING; FORMS; SHUTTERING; BUILDING IMPLEMENTS OR AIDS, OR THEIR USE; HANDLING BUILDING MATERIALS ON THE SITE; REPAIRING, BREAKING-UP OR OTHER WORK ON EXISTING BUILDINGS
    • E04G23/00Working measures on existing buildings
    • E04G23/02Repairing, e.g. filling cracks; Restoring; Altering; Enlarging
    • E04G23/0288Repairing or restoring floor slabs

Landscapes

  • Engineering & Computer Science (AREA)
  • Architecture (AREA)
  • Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Electrochemistry (AREA)
  • Mechanical Engineering (AREA)
  • Civil Engineering (AREA)
  • Structural Engineering (AREA)
  • Reinforcement Elements For Buildings (AREA)

Abstract

本发明公开了一种楼板加固方法,其特征是施工步骤包括:(1)凿除楼板混凝土;(2)在构造柱穿预应力筋和非预应力筋部位钻孔,预应力筋钻孔直径比预应力筋直径大3~4mm,非预应力筋钻孔直径比预应力筋直径大3~4mm;(3)局部剥落构造柱混凝土,露出箍筋后焊接承压钢板;(4)在楼板凿除孔位置安装箍筋、预应力筋、非预应力筋,箍筋与楼板钢筋焊接,抗剪筋嵌入楼板凹槽,楼板凹槽采用环氧树脂砂浆进行封闭;(5)浇筑混凝土;(6)预应力张拉;(7)张拉端封锚。

Description

楼板加固方法
技术领域
本发明涉及建筑领域,特别涉及一种楼板加固方法。
背景技术
楼板在承载力不够时要进行加固,但是加固结构往往难以与原有结构形成整体,主要原因是原有混凝土楼板与加固结构在受力时变形不能协同一致,从而导致混凝土楼板与加固结构受力时不能共同承载,在承受较大荷载是混凝土楼板或者加固结构会出现开裂,加固效果不能体现。可以设置加固梁,提前在加固梁中施加预压力,使其能够产生平衡荷载效应,用以平衡全部或部分结构荷载产生的不利效应。通过施加预应力有效地延缓了楼板裂缝的产生同时减小了楼板的整体挠度。
发明内容
本发明的目的在于提供一种承载力不够的楼板加固方法来解决加固效果不好的问题。
本发明在楼板下面布置横向加固梁和纵向加固梁,横向加固梁和纵向加固梁高度相同,根据加固梁的受力特点,下部处于受拉状态为主要承力部位,加固梁下部进行加强,截面形状采用墩形,截面上部为矩形,截面下部为梯形,矩形高度与楼板厚度相同,矩形宽度为150~200mm,梯形底部长度为200~250mm,梯形高度为120~230mm。横向加固梁和纵向加固梁计算挠度控制为1/300~1/400跨度,这里跨度是指相邻排加固梁的距离。加固梁下部布置预应力筋和非预应力筋,非预应力筋在离梁端0.1跨度部位弯起,这里跨度是指构造柱与第一排纵向加固梁的长度,目的是为了应对上部负弯矩的需要,由于加固结构嵌入构造柱后形成嵌固结构,反弯点位置为0.1跨度,预应力筋或非预应力筋穿过构造柱的钻孔后用环氧树脂植筋胶填塞空隙。预应力筋通长布置,预应力筋穿过构造柱的钻孔后用锚具固定在承压钢板,由于在预应力张拉时构造柱局部会受到很大的压力,承压钢板目的是避免构造柱在张拉时局部承压破坏。非预应力筋布置在加固梁的中部位置,预应力筋布置在加固梁的边部位置。为了满足加固梁的抗剪需要,加固梁设置抗剪筋,抗剪筋设置范围为离加固梁端部5cm位置至加固梁1/3跨度位置,抗剪筋间距为75~100mm,这里跨度是指相邻排加固梁的距离。抗剪筋做成带翼边U形,抗剪筋直径为14~18mm,翼边长度为350~500mm。
施工步骤包括:
(1)凿除楼板混凝土
在加固梁位置凿除楼板混凝土,在放置抗剪筋位置设置凹槽,将楼板底面凿毛以利于与新混凝土形成整体。
(2)在构造柱穿预应力筋和非预应力筋部位钻孔,预应力筋钻孔直径比预应力筋直径大3~4mm,非预应力筋钻孔直径比预应力筋直径大3~4mm。
(3)局部剥落构造柱混凝土,露出箍筋后焊接承压钢板。
(4)在楼板凿除孔位置安装箍筋、预应力筋、非预应力筋,箍筋与楼板钢筋焊接,抗剪筋嵌入楼板凹槽,楼板凹槽采用环氧树脂砂浆进行封闭。
(5)浇筑混凝土
楼板底面涂刷胶水后再进行浇筑混凝土。
(6)预应力张拉
张拉顺序为:先张拉边部的加固梁,再张拉中部的加固梁,张拉采用对称张拉;先张拉横向加固梁,再张拉纵向加固梁。
为减少预应力损失,组装锚具后用预紧器预应紧,千斤顶使用弹簧顶压器,并超张拉5%。为方便施工,两侧张拉端同时进行锚具组装,一端张拉至控制应力后,另一端再补拉至控制应力。
张拉工艺采用如下:第一次张拉至预应力控制值的20%,第二次张拉至预应力控制值,张拉至预应力控制值持续5min后再进行张拉端封锚。
为验证张拉工艺的可行性,确保安全,正式张拉前进行试拉并测试摩擦损失和张拉端预应力筋锚固回缩量。摩擦损失测试采用油压表法,测试时装上千斤顶,但不安装锚具;将千斤顶拉出少许,关上回油阀,然后开动张拉端千斤顶进行张拉;当预应力筋达到张拉力时,分别读出两端千斤顶的油压,即可求得摩擦损失。在张拉过程中测量张拉端预应力筋锚固回缩量。表1为某工程的不同张拉工艺的摩擦损失和张拉端预应力筋锚固回缩量情况,表中反映一次张拉与二次张拉效果有明显的不同,不同二次张拉效果也有差别,“第一次张拉至预应力控制值的20%,第二次张拉至预应力控制值”这个张拉工艺效果最好。
表1不同张拉工艺的摩擦损失和张拉端预应力筋锚固回缩量情况
(7)张拉端封锚
用锚具固定在承压钢板,锚具及预应力筋除油后,表面涂刷环氧树脂两道。
本发明具有力学性能好、安全可靠的优点,具有较好的应用前景。
附图说明
图1为加固梁平面示意图,图2为加固梁截面示意图。
附图标志:1、加固梁,2、预应力筋,3、非预应力筋,4、抗剪筋,5、承压钢板,6、锚具,7、楼板,8、构造柱。
具体实施方式
以下结合附图对本实施例进行详细描述。
本实施例在楼板7下面布置横向加固梁和纵向加固梁,横向加固梁和纵向加固梁高度相同,截面形状采用墩形,截面上部为矩形,截面下部为梯形,矩形高度与楼板7厚度相同,矩形宽度为180mm,梯形底部长度为220mm,梯形高度为180mm。横向加固梁和纵向加固梁计算挠度控制为1/350跨度。加固梁1下部布置预应力筋2和非预应力筋3,非预应力筋3在离梁端0.1跨度部位弯起,预应力筋2或非预应力筋3穿过构造柱8的钻孔后用环氧树脂植筋胶填塞空隙。预应力筋2通长布置,预应力筋2穿过构造柱8的钻孔后用锚具6固定在承压钢板5。非预应力筋3布置在加固梁1的中部位置,预应力筋2布置在加固梁1的边部位置。加固梁1设置抗剪筋4,抗剪筋4设置范围为离加固梁1端部5cm位置至加固梁1/3跨度位置,抗剪筋4间距为100mm。抗剪筋4做成带翼边U形,抗剪筋4直径为16mm,翼边长度为400mm。
施工步骤包括:
(1)凿除楼板7混凝土
在加固梁1位置凿除楼板7混凝土,在放置抗剪筋4位置设置凹槽,将楼板7底面凿毛以利于与新混凝土形成整体。
(2)在构造柱8穿预应力筋2和非预应力筋3部位钻孔,预应力筋2钻孔直径比预应力筋2直径大3mm,非预应力筋3钻孔直径比预应力筋2直径大3mm。
(3)局部剥落构造柱8混凝土,露出箍筋后焊接承压钢板5。
(4)在楼板7凿除孔位置安装箍筋、预应力筋2、非预应力筋3,箍筋与楼板7钢筋焊接,抗剪筋4嵌入楼板7凹槽,楼板7凹槽采用环氧树脂砂浆进行封闭。
(5)浇筑混凝土
楼板7底面涂刷胶水后再进行浇筑混凝土。
(6)预应力张拉
张拉顺序为:先张拉边部的加固梁1,再张拉中部的加固梁1,张拉采用对称张拉;先张拉横向加固梁,再张拉纵向加固梁。
组装锚具6后用预紧器预应紧,千斤顶使用弹簧顶压器,并超张拉5%。两侧张拉端同时进行锚具6组装,一端张拉至控制应力后,另一端再补拉至控制应力。
张拉工艺采用如下:第一次张拉至预应力控制值的20%,第二次张拉至预应力控制值,张拉至预应力控制值持续5min后再进行张拉端封锚。
(7)张拉端封锚
用锚具6固定在承压钢板5,锚具6及预应力筋2除油后,表面涂刷环氧树脂两道。

Claims (3)

1.一种楼板加固方法,其特征是施工步骤包括:
(1)凿除楼板混凝土
在加固梁位置凿除楼板混凝土,在放置抗剪筋位置设置凹槽,将楼板底面凿毛以利于与新混凝土形成整体;
(2)在构造柱穿预应力筋和非预应力筋部位钻孔,预应力筋钻孔直径比预应力筋直径大3~4mm,非预应力筋钻孔直径比预应力筋直径大3~4mm;
(3)局部剥落构造柱混凝土,露出箍筋后焊接承压钢板;
(4)在楼板凿除孔位置安装箍筋、预应力筋、非预应力筋,箍筋与楼板钢筋焊接,抗剪筋嵌入楼板凹槽,楼板凹槽采用环氧树脂砂浆进行封闭;
(5)浇筑混凝土
楼板底面涂刷胶水后再进行浇筑混凝土;
(6)预应力张拉
张拉顺序为:先张拉边部的加固梁,再张拉中部的加固梁,张拉采用对称张拉;先张拉横向加固梁,再张拉纵向加固梁;
组装锚具后用预紧器预应紧,千斤顶使用弹簧顶压器,并超张拉5%;两侧张拉端同时进行锚具组装,一端张拉至控制应力后,另一端再补拉至控制应力;
张拉工艺采用如下:第一次张拉至预应力控制值的20%,第二次张拉至预应力控制值,张拉至预应力控制值持续5min后再进行张拉端封锚;
(7)张拉端封锚
用锚具固定在承压钢板,锚具及预应力筋除油后,表面涂刷环氧树脂两道。
2.根据权利要求1所述的承载力不够的楼板加固方法,其特征是抗剪筋设置范围为离加固梁端部5cm位置至加固梁1/3跨度位置,抗剪筋间距为75~100mm。
3.根据权利要求2所述的承载力不够的楼板加固方法,其特征是抗剪筋做成带翼边U形,抗剪筋直径为14~18mm,翼边长度为350~500mm。
CN201710721872.0A 2016-03-02 2016-03-02 楼板加固方法 Pending CN107269023A (zh)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201710721872.0A CN107269023A (zh) 2016-03-02 2016-03-02 楼板加固方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
CN201610181706.1A CN105781139B (zh) 2016-03-02 2016-03-02 承载力不够的楼板加固方法
CN201710721872.0A CN107269023A (zh) 2016-03-02 2016-03-02 楼板加固方法

Related Parent Applications (1)

Application Number Title Priority Date Filing Date
CN201610181706.1A Division CN105781139B (zh) 2016-03-02 2016-03-02 承载力不够的楼板加固方法

Publications (1)

Publication Number Publication Date
CN107269023A true CN107269023A (zh) 2017-10-20

Family

ID=56391975

Family Applications (2)

Application Number Title Priority Date Filing Date
CN201710721872.0A Pending CN107269023A (zh) 2016-03-02 2016-03-02 楼板加固方法
CN201610181706.1A Expired - Fee Related CN105781139B (zh) 2016-03-02 2016-03-02 承载力不够的楼板加固方法

Family Applications After (1)

Application Number Title Priority Date Filing Date
CN201610181706.1A Expired - Fee Related CN105781139B (zh) 2016-03-02 2016-03-02 承载力不够的楼板加固方法

Country Status (1)

Country Link
CN (2) CN107269023A (zh)

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN109162398A (zh) * 2018-09-26 2019-01-08 中建科技(深汕特别合作区)有限公司 双向预应力密肋楼板构件及双向预应力密肋楼板
CN110593142A (zh) * 2019-09-21 2019-12-20 北京凯新浩达工程技术有限公司 一种桥梁修复方法
CN110836023A (zh) * 2017-09-12 2020-02-25 叶长青 一种混凝土梁的加固施工方法
CN114776070A (zh) * 2022-04-25 2022-07-22 兰州有色冶金设计研究院有限公司 一种大跨度楼板的加固结构及方法

Families Citing this family (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN106437192B (zh) * 2016-10-21 2018-10-16 江苏东南特种技术工程有限公司 一种在板面采用预应力拉索加固的方法
CN107327157B (zh) * 2017-09-04 2023-12-15 安徽津达建材股份有限公司 混凝土楼板加固结构
CN108343259A (zh) * 2018-02-06 2018-07-31 广东省基础工程集团有限公司 一种预应力加固梁及其施工方法
CN109469349A (zh) * 2018-11-19 2019-03-15 中国矿业大学 一种增设钢筋混凝土次梁的楼板加固改造方法
CN111287486B (zh) * 2020-02-19 2021-06-22 浙江固邦建筑特种技术有限公司 一种空心楼板托换为现浇楼板的施工方法

Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008115584A (ja) * 2006-11-02 2008-05-22 Penta Ocean Construction Co Ltd 鉄筋コンクリート構造物の補強方法
CN202787099U (zh) * 2012-07-12 2013-03-13 江祥林 加固混凝土盖梁的体外预应力结构
CN202969979U (zh) * 2012-11-28 2013-06-05 南京固强建筑技术有限公司 抽柱施工加固结构
CN103321444A (zh) * 2013-06-14 2013-09-25 罗海军 混凝土楼板加固施工方法
JP2014092005A (ja) * 2012-11-06 2014-05-19 Takenaka Komuten Co Ltd 有孔梁の補強構造
CN104818861A (zh) * 2013-08-03 2015-08-05 叶香竹 预应力加固楼板方法
CN104878835A (zh) * 2015-05-19 2015-09-02 叶长青 条形基础房屋后增地下室结构

Family Cites Families (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2809085B2 (ja) * 1994-02-01 1998-10-08 鹿島建設株式会社 鉄筋コンクリート床スラブの補強方法
AU2001273296A1 (en) * 2000-07-10 2002-01-21 The Regents Of The University Of Michigan Concrete construction employing the use of a ductile strip
CN101871267B (zh) * 2010-06-30 2011-08-31 西南科技大学 老化钢筋混凝土梁复合加固工艺
CN104060849A (zh) * 2014-07-05 2014-09-24 刘广义 混凝土空心板的凿孔叠合加固方法
CN204098523U (zh) * 2014-09-24 2015-01-14 安徽天筑建设(集团)有限公司 一种钢筋混凝土楼板后开洞加梁补强结构

Patent Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008115584A (ja) * 2006-11-02 2008-05-22 Penta Ocean Construction Co Ltd 鉄筋コンクリート構造物の補強方法
CN202787099U (zh) * 2012-07-12 2013-03-13 江祥林 加固混凝土盖梁的体外预应力结构
JP2014092005A (ja) * 2012-11-06 2014-05-19 Takenaka Komuten Co Ltd 有孔梁の補強構造
CN202969979U (zh) * 2012-11-28 2013-06-05 南京固强建筑技术有限公司 抽柱施工加固结构
CN103321444A (zh) * 2013-06-14 2013-09-25 罗海军 混凝土楼板加固施工方法
CN104818861A (zh) * 2013-08-03 2015-08-05 叶香竹 预应力加固楼板方法
CN104878835A (zh) * 2015-05-19 2015-09-02 叶长青 条形基础房屋后增地下室结构

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN110836023A (zh) * 2017-09-12 2020-02-25 叶长青 一种混凝土梁的加固施工方法
CN109162398A (zh) * 2018-09-26 2019-01-08 中建科技(深汕特别合作区)有限公司 双向预应力密肋楼板构件及双向预应力密肋楼板
CN110593142A (zh) * 2019-09-21 2019-12-20 北京凯新浩达工程技术有限公司 一种桥梁修复方法
CN114776070A (zh) * 2022-04-25 2022-07-22 兰州有色冶金设计研究院有限公司 一种大跨度楼板的加固结构及方法

Also Published As

Publication number Publication date
CN105781139A (zh) 2016-07-20
CN105781139B (zh) 2017-12-15

Similar Documents

Publication Publication Date Title
CN105781139B (zh) 承载力不够的楼板加固方法
US11293183B2 (en) Precast column base joint and construction method therefor
US10640977B2 (en) Concrete structure using reinforcing panel including embedded reinforcing grid and method of repairing and reinforcing the same
CN207017144U (zh) 一种用于全预制拼装桥墩的连接结构
KR100899372B1 (ko) 기존 콘크리트 기초구조물로의 새로운 마이크로파일 두부의정착 방법 및 이를 이용한 기초 및 기둥 구조물의 보강공법 및 그 보강 구조
KR100952207B1 (ko) 프리캐스트 교각과 기초의 연결구조 및 연결시공방법
CN109057392B (zh) 一种加固用钢结构施工方法
Singhal et al. Anchorage behaviour of headed bars as connection system for precast reinforced concrete structural components
CN102979221A (zh) 一种配置交叉斜向体内预应力的剪力墙结构及其施工方法
CN102926483A (zh) 一种自恢复、耗能、易修复的混合装配式混凝土剪力墙
CN210562163U (zh) 一种预制预应力锚杆杆件
CN104806031B (zh) 木结构加固施工方法
JP4834890B2 (ja) プレキャストコンクリート部材間の間詰め部に対するプレストレス導入方法
Chourasia et al. Influential parameters for headed bars in RC beam-column joint
CN110747735A (zh) 钢-混凝土组合梁预制混凝土桥面板的锚固连接装置
KR20100053846A (ko) 표면매립 긴장공법의 구조물 충전장치 및 충전 방법
CN212404845U (zh) 一种连续梁桥墩梁临时固结系统和连续梁桥
KR100462925B1 (ko) 외부 강선을 이용한 교량의 보강 공법 및 그에 적용되는강재정착물
RU2468143C2 (ru) Сталежелезобетонное пролетное строение моста и способ его изготовления
KR101197318B1 (ko) 휨 연결재를 이용한 프리캐스트 프리스트레스 콘크리트 빔의 연결부 보강방법 및 이를 이용한 교량시공방법
KR101535180B1 (ko) 교량상부구조용 콘크리트거더
CN111411625A (zh) 一种锚杆的后张预应力施加装置
KR100549044B1 (ko) 콘크리트 구조물의 인장력을 받는 단면에 대한 내하력보강을 위한 인장부 보수보강장치 및 이의 설치방법
KR100530025B1 (ko) 확대된 단면에 프리스트레스를 도입하여 철근 콘크리트구조물의 지지력 보강을 위한 단면 확대 보수보강장치 및이를 이용한 보수보강 시공방법
CN106592839A (zh) 一种横张体外预应力压型钢板组合楼板

Legal Events

Date Code Title Description
PB01 Publication
PB01 Publication
SE01 Entry into force of request for substantive examination
SE01 Entry into force of request for substantive examination
RJ01 Rejection of invention patent application after publication

Application publication date: 20171020