CN105200649A - 一种高厚实感涤纶拉舍尔毛毯的生产工艺 - Google Patents

一种高厚实感涤纶拉舍尔毛毯的生产工艺 Download PDF

Info

Publication number
CN105200649A
CN105200649A CN201510501195.2A CN201510501195A CN105200649A CN 105200649 A CN105200649 A CN 105200649A CN 201510501195 A CN201510501195 A CN 201510501195A CN 105200649 A CN105200649 A CN 105200649A
Authority
CN
China
Prior art keywords
groove
grey cloth
washing
polyester
clear water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510501195.2A
Other languages
English (en)
Inventor
胡永伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Wuxi world Agel Ecommerce Ltd
Original Assignee
DAJIN BIANWU (WUXI) Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by DAJIN BIANWU (WUXI) Co Ltd filed Critical DAJIN BIANWU (WUXI) Co Ltd
Priority to CN201510501195.2A priority Critical patent/CN105200649A/zh
Publication of CN105200649A publication Critical patent/CN105200649A/zh
Pending legal-status Critical Current

Abstract

本发明公开一种高厚实感涤纶拉舍尔毛毯的生产工艺,包括以下步骤:a、选料;b、织造;c、坯布定型;d、烫光;e、印花或染色;f、一次烘干;g、蒸化;h、水洗;i、二次烘干;j、整理;k、成品定型。本发明生产出的毛毯与传统工艺生产出的毛毯相比,在同等重量的前提下,其厚实感与绒面丰满度更高,且绒面更为平整、精细,更具观赏性与保暖性。

Description

一种高厚实感涤纶拉舍尔毛毯的生产工艺
技术领域
本发明涉及毛毯的生产工艺,尤其涉及一种高厚实感涤纶拉舍尔毛毯的生产工艺。
背景技术
毛毯是一种常用的床上用品,具有保暖功能,其表面有丰厚的毛绒。现有市场上的毛毯,都是采用16E或18E或20E的经编机织造而成,且在织造时,选用的是横向跨度较小的三针或四针衬围,然而,随着消费者对毛毯要求的越来越高,对于毛毯的厚实度及绒面丰满度就提出了更高的要求,现有做法是通过增加原材料的投入来实现毛毯厚实度及绒面丰满度的提高,此种方式大大增加了生产成本,由此,急需解决。
发明内容
本发明的目的在于针对上述问题,提供一种在同等重量时厚实度及绒面丰满度优于常规毛毯的涤纶拉舍尔毛毯生产工艺。
本发明的目的是通过以下技术方案来实现:
一种高厚实感涤纶拉舍尔毛毯的生产工艺,包括以下步骤:
a、选料:毛毯的底布选择200D涤纶FDY、150D涤纶FDY、100D涤纶FDY中的任意两种混合搭配,毛毯的绒面选择200D涤纶DTY;
b、织造:在14E经编机上采用五把导纱梳栉编织而成;
c、坯布定型:将织造好的坯布在定型机上进行定型;
d、烫光:对定型后的坯布进行烫光;
e、印花或染色:将织造出的坯布印花或染色;
f、一次烘干:对印花或染色的坯布进行烘干;
g、蒸化:对坯布进行蒸化;
h、水洗:对蒸化后的坯布进行多槽水洗;
i、二次烘干:对水洗后的坯布进行烘干,烘干后冷却至常温;
j、整理:对坯布进行刷毛、起毛、烫剪;
k、成品定型:裁剪并缝制成相应规格的成品。
作为本发明的一种优选方案,所述步骤f、步骤i在烘箱中进行烘干,烘干温度为150℃。
作为本发明的一种优选方案,所述步骤c中定型温度控制在100~135℃。
作为本发明的一种优选方案,所述步骤e中采用十槽水洗,第一槽为常温清水水洗,第二槽为常温皂洗,第三槽为常温皂洗,第四槽为常温皂洗,第五槽为在20~70℃下清水水洗,第六槽为在20~70℃下清水水洗,第七槽为在20~70℃下清水水洗,第八槽为在20~70℃下清水水洗,第九槽为在20~70℃下清水水洗,第十槽为常温添加柔软整理剂水洗。
本发明的有益效果为:所述一种高厚实感涤纶拉舍尔毛毯的生产工艺其底布采用200D涤纶FDY、150D涤纶FDY、100D涤纶FDY中的任意两种混合搭配,绒面采用200D涤纶DTY,并选用14E经编机配五把导纱梳栉进行编织,使得其织造密度更大,后经坯布定型、烫光、印花或染色、一次烘干、蒸化、水洗、二次烘干、整理、成品定型等工艺,生产出的毛毯与传统工艺生产出的毛毯相比,在同等重量的前提下,其厚实感与绒面丰满度更高,且绒面更为平整、精细,更具观赏性与保暖性。
具体实施方式
下面结合通过具体实施方式来进一步说明本发明的技术方案。
实施例1:200*240*6KG双层涤纶印花毛毯
于本实施例中,一种高厚实感涤纶拉舍尔毛毯的生产工艺,包括以下步骤:
a、选料:毛毯的底布选择200D涤纶FDY、150D涤纶FDY混合搭配,毛毯的绒面选择200D涤纶DTY;
b、织造:在14E经编机上采用五把导纱梳栉编织而成,机上隔距为20mm,毛坯设定幅宽为228cm,上机盘头根数为320根*4,牵拉密度为11.5毫米/圈,CB1为6.34毫米/圈,CB2为3.87毫米/圈,CB3为48.04毫米/圈,CB4为3.87毫米/圈,CB5为6.34毫米/圈;
c、坯布定型:将织造好的坯布在定型机上进行定型,门幅为220cm,定型温度为100℃;
d、烫光:对定型后的坯布进行烫光;
e、印花或染色:将织造出的坯布印花或染色;
f、一次烘干:采用烘箱对印花或染色的坯布进行烘干,烘干温度为150℃;
g、蒸化:对坯布进行蒸化;
h、水洗:对蒸化后的坯布进行十槽水洗,第一槽为常温清水水洗,第二槽为常温皂洗,第三槽为常温皂洗,第四槽为常温皂洗,第五槽为在20℃下清水水洗,第六槽为在20℃下清水水洗,第七槽为在20℃下清水水洗,第八槽为在20℃下清水水洗,第九槽为在20℃下清水水洗,第十槽为常温添加柔软整理剂水洗;
i、二次烘干:采用烘箱对水洗后的坯布进行烘干,烘干温度为150℃,烘干后冷却至常温;
j、整理:对坯布进行刷毛、起毛、烫剪;
k、成品定型:裁剪并缝制成相应规格的成品。
采用上述工艺生产的6KG双层涤纶印花毛毯,其成品毛高可达到7.5~8mm,其可达到常规16E、18E、20E所生产双层涤纶印花毛毯200*240*7.5KG的厚实感与绒面丰满度,且绒面更为平整、精细,更具观赏性与保暖性,有效地在节省原料的同时又提升了产品的品质。
实施例2200*240*3.0KG单层涤纶印花毛毯
于本实施例中,于本实施例中,一种高厚实感涤纶拉舍尔毛毯的生产工艺,包括以下步骤:
a、选料:毛毯的底布选择200D涤纶FDY、150D涤纶FDY混合搭配,毛毯的绒面选择200D涤纶DTY;
b、织造:在14E经编机上采用五把导纱梳栉编织而成,隔距为18mm,坯布设定幅宽为218cm,上机盘头根数为310根*4,牵拉密度为12毫米/圈,CB1为7.34毫米/圈,CB2为3.75毫米/圈,CB3为44.9毫米/圈,CB4为3.75毫米/圈,CB5为7.34毫米/圈;
c、坯布定型:将织造好的坯布在定型机上进行定型,门幅为218cm,定型温度为120℃;
d、烫光:对定型后的坯布进行烫光;
e、印花或染色:将织造出的坯布印花或染色;
f、一次烘干:采用烘箱对印花或染色的坯布进行烘干,烘干温度为150℃;
g、蒸化:对坯布进行蒸化;
h、水洗:对蒸化后的坯布进行十槽水洗,第一槽为常温清水水洗,第二槽为常温皂洗,第三槽为常温皂洗,第四槽为常温皂洗,第五槽为在45℃下清水水洗,第六槽为在45℃下清水水洗,第七槽为在45℃下清水水洗,第八槽为在45℃下清水水洗,第九槽为在45℃下清水水洗,第十槽为常温添加柔软整理剂水洗;
i、二次烘干:采用烘箱对水洗后的坯布进行烘干,烘干温度为150℃,烘干后冷却至常温;
j、整理:对坯布进行刷毛、起毛、烫剪;
k、成品定型:裁剪并缝制成相应规格的成品。
采用上述工艺生产的200*240*3KG单层涤纶印花毛毯,其成品毛高可达到7~7.5mm,其可达常规16针、18针生产的单层涤纶毛毯同等规格:3.5kg~4kg的厚实度与绒面丰满度,且绒面更为平整、精细,更具观赏性与实用性,有效地节省原料的同时提升了产品的品质。
实施例3200*240*4.0KG双层涤纶印花毛毯
于本实施例中,于本实施例中,一种高厚实感涤纶拉舍尔毛毯的生产工艺,包括以下步骤:
a、选料:毛毯的底布选择150D涤纶FDY、100D涤纶FDY混合搭配,毛毯的绒面选择200D涤纶DTY;
b、织造:在14E经编机上采用五把导纱梳栉编织而成,隔距为18mm,坯布设定幅宽为218cm,上机盘头315根*4,牵拉密度为9.5毫米/圈,CB1为7.34毫米/圈,CB2为4.18毫米/圈,CB3为44.9毫米/圈,CB4为4.418毫米/圈,CB5为7.34毫米/圈;
c、坯布定型:将织造好的坯布在定型机上进行定型,门幅为218mm,定型温度为135℃;
d、烫光:对定型后的坯布进行烫光;
e、印花或染色:将织造出的坯布印花或染色;
f、一次烘干:采用烘箱对印花或染色的坯布进行烘干,烘干温度为150℃;
g、蒸化:对坯布进行蒸化;
h、水洗:对蒸化后的坯布进行十槽水洗,第一槽为常温清水水洗,第二槽为常温皂洗,第三槽为常温皂洗,第四槽为常温皂洗,第五槽为在70℃下清水水洗,第六槽为在70℃下清水水洗,第七槽为在70℃下清水水洗,第八槽为在70℃下清水水洗,第九槽为在70℃下清水水洗,第十槽为常温添加柔软整理剂水洗;
i、二次烘干:采用烘箱对水洗后的坯布进行烘干,烘干温度为150℃,烘干后冷却至常温;
j、整理:对坯布进行刷毛、起毛、烫剪;
k、成品定型:裁剪并缝制成相应规格的成品。
采用以上工艺生产的200*240*4.0KG双层涤纶印花毛毯,其成品毛高可达到7~7.5mm,其可达到常规16针、18针所生产的双层涤纶印花毛毯200*240*5KG的厚实感与绒面丰满度,且绒面更为平整、精细、更具观赏性与实用性,有效地节省原料的同时提升了产品的品质。
以上实施例只是阐述了本发明的基本原理和特性,本发明不受上述实施例限制,在不脱离本发明精神和范围的前提下,本发明还有各种变化和改变,这些变化和改变都纳入要求保护的本发明范围内。本发明要求保护范围由所附的权利要求书及其等效物界定。

Claims (4)

1.一种高厚实感涤纶拉舍尔毛毯的生产工艺,其特征在于:包括以下步骤:
a、选料:毛毯的底布选择200D涤纶FDY、150D涤纶FDY、100D涤纶FDY中的任意两种混合搭配,毛毯的绒面选择200D涤纶DTY;
b、织造:在14E经编机上采用五把导纱梳栉编织而成;
c、坯布定型:将织造好的坯布在定型机上进行定型;
d、烫光:对定型后的坯布进行烫光;
e、印花或染色:将织造出的坯布印花或染色;
f、一次烘干:对印花或染色的坯布进行烘干;
g、蒸化:对坯布进行蒸化;
h、水洗:对蒸化后的坯布进行多槽水洗;
i、二次烘干:对水洗后的坯布进行烘干,烘干后冷却至常温;
j、整理:对坯布进行刷毛、起毛、烫剪;
k、成品定型:裁剪并缝制成相应规格的成品。
2.根据权利要求1所述的一种高厚实感涤纶拉舍尔毛毯的生产工艺,其特征在于:所述步骤f、步骤i在烘箱中进行烘干,烘干温度为150℃。
3.根据权利要求1所述的一种高厚实感涤纶拉舍尔毛毯的生产工艺,其特征在于:所述步骤c中定型温度控制在100~135℃。
4.根据权利要求1所述的一种高厚实感涤纶拉舍尔毛毯的生产工艺,其特征在于:所述步骤e中采用十槽水洗,第一槽为常温清水水洗,第二槽为常温皂洗,第三槽为常温皂洗,第四槽为常温皂洗,第五槽为在20~70℃下清水水洗,第六槽为在20~70℃下清水水洗,第七槽为在20~70℃下清水水洗,第八槽为在20~70℃下清水水洗,第九槽为在20~70℃下清水水洗,第十槽为常温添加柔软整理剂水洗。
CN201510501195.2A 2015-08-14 2015-08-14 一种高厚实感涤纶拉舍尔毛毯的生产工艺 Pending CN105200649A (zh)