CN104016719A - Reactive crystalline glaze with sagging effect and preparation method of reactive crystalline glaze - Google Patents

Reactive crystalline glaze with sagging effect and preparation method of reactive crystalline glaze Download PDF

Info

Publication number
CN104016719A
CN104016719A CN201410200111.7A CN201410200111A CN104016719A CN 104016719 A CN104016719 A CN 104016719A CN 201410200111 A CN201410200111 A CN 201410200111A CN 104016719 A CN104016719 A CN 104016719A
Authority
CN
China
Prior art keywords
parts
coat enamel
glaze
ground
cover
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410200111.7A
Other languages
Chinese (zh)
Other versions
CN104016719B (en
Inventor
王智永
林保春
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
TOP COLLECTION CO Ltd
Original Assignee
TOP COLLECTION CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TOP COLLECTION CO Ltd filed Critical TOP COLLECTION CO Ltd
Priority to CN201410200111.7A priority Critical patent/CN104016719B/en
Publication of CN104016719A publication Critical patent/CN104016719A/en
Application granted granted Critical
Publication of CN104016719B publication Critical patent/CN104016719B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a reactive crystalline glaze with a sagging effect. The glaze comprises a ground glaze and a surface glaze, wherein the ground glaze comprises the following components in parts by mass: 25-35 parts of feldspar, 20-23 parts of quartz, 10-12 parts of calcite, 3-5 parts of Guizhou soil, 5-8 parts of zinc oxide, 8-10 parts of titanium oxide, 8-10 parts of zirconium silicate, 7-11 parts of barium carbonate and 6-8 parts of wollastonite; the surface glaze comprises the following components in parts by mass: 23-25 parts of feldspar, 12-15 parts of quartz, 10-15 parts of calcite, 6-8 parts of Guizhou soil, 12-15 parts of zinc oxide, 8-10 parts of zirconium silicate and 11-15 parts of chromophore. The glaze disclosed by the invention has the effects of crystallization and sagging to ensure that the whole glaze is more colorful.

Description

There is reactive crystallization glaze of sagging effect and preparation method thereof
Technical field
The present invention relates to a kind of reactive crystallization glaze with sagging effect and preparation method thereof.
Background technology
At present, in ceramic industry, the moulding of porcelain base is that the allotment of the basic glaze of quality products makes porcelain more dazzling brilliant, the porcelain base of same moulding, often because glaze is different, and makes human consumer's vision produce different impacts, that can present crystallization, the glaze again with sagging effect, gives the porcelain of a kind of magnificent perception of people, product when this is also current porcelain industry a kind of.
Summary of the invention
Technical problem to be solved by this invention is to overcome the deficiencies in the prior art, and a kind of reactive crystallization glaze with sagging effect is provided, and its existing crystallization effect of glaze has again the effect of sagging, makes whole glaze more colorful.
In order to solve the problems of the technologies described above, technical scheme of the present invention is: a kind of reactive crystallization glaze with sagging effect, comprise ground-coat enamel and cover-coat enamel, and the component of described ground-coat enamel and each component mass parts are as follows: feldspar: 25 parts~35 parts; Quartzy: 20 parts~23 parts; Calcite: 10 parts~12 parts; Guizhou clay: 3 parts~5 parts; Zinc oxide: 5 parts~8 parts; Titanium oxide: 8 parts~10 parts; Zirconium silicate: 8 parts~10 parts; Barium carbonate: 7 parts~11 parts; Wollastonite: 6 parts~8 parts; The component of described cover-coat enamel and each component mass parts are as follows: feldspar: 23 parts~25 parts; Quartzy: 12 parts~15 parts; Calcite: 10 parts~15 parts; 6 parts~8 parts of Guizhou clays; Zinc oxide: 12 parts~15 parts; Zirconium silicate: 8 parts~10 parts; Color base: 11 parts~15 parts.
The present invention also provides a kind of this to have the making method of the reactive crystallization glaze of sagging effect, and the step of the method is as follows:
A) according to each component and each component mass parts, get the raw materials ready:
B) ground-coat enamel is pressed ground-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 10~12 hours, and the glaze after ball milling is crossed after 160 mesh sieves, then the ground-coat enamel of furnishing 50~70 degree Beaume slurry, gets the bright and clean base substrate of appearance and immerses this ground-coat enamel slurry, dry rear stand-by;
C) cover-coat enamel is pressed cover-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 11~13 hours, the glaze after ball milling is crossed after 160 mesh sieves, then the cover-coat enamel of furnishing 50~70 degree Beaume slurry, the base substrate of upper base glaze slip is sprayed to this cover-coat enamel slurry, under the oxidizing atmosphere of 1160~1200 ℃, fire finished product.
Adopted after technique scheme, by adopting new technology, make and make the collocation of reactive crystallization glaze and sagging decorate more stable, by double-deck reaction effect, make glaze present crystallization effect, add sagging effect simultaneously, make dull glaze more lively, make glaze seem more splendid, make glaze colorful, to people, feel, neither complicated ugly, can simply not show dull again, and burn till fast in the roller kiln of 1160~1200 ℃, make glaze novel, and firing range is wide, glaze is attractive in appearance, do things creatively, be well received by consumers.
Embodiment
For content of the present invention is more easily expressly understood, below according to specific embodiment, the present invention is further detailed explanation.
Embodiment mono-
A reactive crystallization glaze with sagging effect, comprises ground-coat enamel and cover-coat enamel, and the component of described ground-coat enamel and each component mass parts are as follows: feldspar: 35 parts; Quartzy: 23 parts; Calcite: 12 parts; Guizhou clay: 5 parts; Zinc oxide: 5 parts; Titanium oxide: 10 parts; Zirconium silicate: 10 parts; Barium carbonate: 11 parts; Wollastonite: 8 parts; The component of cover-coat enamel and each component mass parts are as follows: feldspar: 25 parts; Quartzy: 15 parts; Calcite: 15 parts; 8 parts of Guizhou clays; Zinc oxide: 15 parts; Zirconium silicate: 10 parts; Color base: 15 parts.
This has the making method of the reactive crystallization glaze of sagging effect, and the step of the method is as follows:
A) according to each component and each component mass parts, get the raw materials ready:
B) ground-coat enamel is pressed ground-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, and wet ball grinding is about 11 hours, and the glaze after ball milling is crossed after 160 mesh sieves, then the ground-coat enamel of furnishing 50~70 degree Beaume slurry, gets the bright and clean base substrate of appearance and immerses this ground-coat enamel slurry, dry rear stand-by;
C) cover-coat enamel is pressed cover-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, about wet ball grinding 12 hours, the glaze after ball milling is crossed after 160 mesh sieves, then the cover-coat enamel of furnishing 50~70 degree Beaume slurry, the base substrate of upper base glaze slip is sprayed to this cover-coat enamel slurry, under the oxidizing atmosphere of 1160~1200 ℃, fire finished product.
Embodiment bis-
A reactive crystallization glaze with sagging effect, comprises ground-coat enamel and cover-coat enamel, and the component of described ground-coat enamel and each component mass parts are as follows: feldspar: 25 parts; Quartzy: 20 parts; Calcite: 10 parts; Guizhou clay: 3 parts; Zinc oxide: 5 parts; Titanium oxide: 8 parts; Zirconium silicate: 8 parts; Barium carbonate: 7 parts; Wollastonite: 6 parts; The component of cover-coat enamel and each component mass parts are as follows: feldspar: 23 parts; Quartzy: 12 parts; Calcite: 10 parts; 6 parts of Guizhou clays; Zinc oxide: 12 parts; Zirconium silicate: 8 parts; Color base: 11 parts.
This has the making method of the reactive crystallization glaze of sagging effect, and the step of the method is as follows:
A) according to each component and each component mass parts, get the raw materials ready:
B) ground-coat enamel is pressed ground-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 10 hours, and the glaze after ball milling is crossed after 160 mesh sieves, then the ground-coat enamel of furnishing 50~70 degree Beaume slurry, gets the bright and clean base substrate of appearance and immerses this ground-coat enamel slurry, dry rear stand-by;
C) cover-coat enamel is pressed cover-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 11 hours, the glaze after ball milling is crossed after 160 mesh sieves, then the cover-coat enamel of furnishing 50~70 degree Beaume slurry, the base substrate of upper base glaze slip is sprayed to this cover-coat enamel slurry, under the oxidizing atmosphere of 1160~1200 ℃, fire finished product.
Embodiment tri-
A reactive crystallization glaze with sagging effect, comprises ground-coat enamel and cover-coat enamel, and the component of described ground-coat enamel and each component mass parts are as follows: feldspar: 30 parts; Quartzy: 21 parts; Calcite: 11 parts; Guizhou clay: 4 parts; Zinc oxide: 7 parts; Titanium oxide: 9 parts; Zirconium silicate: 9 parts; Barium carbonate: 9 parts; Wollastonite: 7 parts; The component of cover-coat enamel and each component mass parts are as follows: feldspar: 24 parts; Quartzy: 13 parts; Calcite: 23 parts; 7 parts of Guizhou clays; Zinc oxide: 14 parts; Zirconium silicate: 9 parts; Color base: 13 parts.
This has the making method of the reactive crystallization glaze of sagging effect, and the step of the method is as follows:
A) according to each component and each component mass parts, get the raw materials ready:
B) ground-coat enamel is pressed ground-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 12 hours, and the glaze after ball milling is crossed after 160 mesh sieves, then the ground-coat enamel of furnishing 50~70 degree Beaume slurry, gets the bright and clean base substrate of appearance and immerses this ground-coat enamel slurry, dry rear stand-by;
C) cover-coat enamel is pressed cover-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 13 hours, the glaze after ball milling is crossed after 160 mesh sieves, then the cover-coat enamel of furnishing 50~70 degree Beaume slurry, the base substrate of upper base glaze slip is sprayed to this cover-coat enamel slurry, under the oxidizing atmosphere of 1160~1200 ℃, fire finished product.
The reactive crystallization glaze with sagging effect prepared by above-mentioned three embodiment, its glaze all presents crystallization effect, all there is sagging effect simultaneously, make dull glaze more lively, make glaze seem more splendid, make glaze colorful, to people, feel, neither complicated ugly, can simply not show dull again.
Above-described specific embodiment; technical problem, technical scheme and beneficial effect that the present invention is solved further describe; institute is understood that; the foregoing is only specific embodiments of the invention; be not limited to the present invention; within the spirit and principles in the present invention all, any modification of making, be equal to replacement, improvement etc., within all should being included in protection scope of the present invention.

Claims (2)

1. a reactive crystallization glaze with sagging effect, comprises ground-coat enamel and cover-coat enamel, it is characterized in that: the component of described ground-coat enamel and each component mass parts are as follows: feldspar: 25 parts~35 parts; Quartzy: 20 parts~23 parts; Calcite: 10 parts~12 parts; Guizhou clay: 3 parts~5 parts; Zinc oxide: 5 parts~8 parts; Titanium oxide: 8 parts~10 parts; Zirconium silicate: 8 parts~10 parts; Barium carbonate: 7 parts~11 parts; Wollastonite: 6 parts~8 parts; The component of described cover-coat enamel and each component mass parts are as follows: feldspar: 23 parts~25 parts; Quartzy: 12 parts~15 parts; Calcite: 10 parts~15 parts; 6 parts~8 parts of Guizhou clays; Zinc oxide: 12 parts~15 parts; Zirconium silicate: 8 parts~10 parts; Color base: 11 parts~15 parts.
2. a making method with the reactive crystallization glaze of sagging effect as claimed in claim 1, is characterized in that the step of the method is as follows:
A) according to each component and each component mass parts, get the raw materials ready:
B) ground-coat enamel is pressed ground-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 10~12 hours, and the glaze after ball milling is crossed after 160 mesh sieves, then the ground-coat enamel of furnishing 50~70 degree Beaume slurry, gets the bright and clean base substrate of appearance and immerses this ground-coat enamel slurry, dry rear stand-by;
C) cover-coat enamel is pressed cover-coat enamel Liao ︰ Qiu ︰ water=1 ︰ 1.5 ︰ 0.5, wet ball grinding 11~13 hours, the glaze after ball milling is crossed after 160 mesh sieves, then the cover-coat enamel of furnishing 50~70 degree Beaume slurry, the base substrate of upper base glaze slip is sprayed to this cover-coat enamel slurry, under the oxidizing atmosphere of 1160~1200 ℃, fire finished product.
CN201410200111.7A 2014-05-13 2014-05-13 Reactive crystallization glaze with sagging effect and preparation method thereof Active CN104016719B (en)