CN103924744A - 一种彩色涂层压花铝板 - Google Patents

一种彩色涂层压花铝板 Download PDF

Info

Publication number
CN103924744A
CN103924744A CN201410124792.3A CN201410124792A CN103924744A CN 103924744 A CN103924744 A CN 103924744A CN 201410124792 A CN201410124792 A CN 201410124792A CN 103924744 A CN103924744 A CN 103924744A
Authority
CN
China
Prior art keywords
enter
aluminium sheet
aluminum plate
degreasing
drying
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410124792.3A
Other languages
English (en)
Other versions
CN103924744B (zh
Inventor
汪厚福
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHEJIANG SAIWANTE TECHNOLOGY Co Ltd
Original Assignee
ZHEJIANG SAIWANTE TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHEJIANG SAIWANTE TECHNOLOGY Co Ltd filed Critical ZHEJIANG SAIWANTE TECHNOLOGY Co Ltd
Priority to CN201410124792.3A priority Critical patent/CN103924744B/zh
Publication of CN103924744A publication Critical patent/CN103924744A/zh
Application granted granted Critical
Publication of CN103924744B publication Critical patent/CN103924744B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明提供了一种彩色涂层压花铝板,其通过包括如下步骤的方法制成:将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油;进入清洗槽内进行清洗;清洗后进入钝化槽钝化,在钝化层上涂上底漆,然后进入烘箱烘干;进入涂装线辊涂,再进入烘箱烘干;经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。本发明的一种彩色涂层压花铝板,使得该产品抗紫外线和耐酸耐碱性能更强。同时,该产品既有彩钢的高强度性能,又有耐腐蚀、美观的优点,可用于屋顶。

Description

一种彩色涂层压花铝板
技术领域
本发明属于建材领域,具体是一种彩色涂层压花铝板。      
背景技术
压花铝板又可以称为铝压花板:属于在铝板的基础上,经过压延加工而在表面形成各种花纹的铝产品,应用较为广泛,主要用在包装,建筑,幕墙等方面。普通的压花铝板,抗紫外线和耐酸耐碱性能不够好,强度和耐腐蚀性也不够好,不适合用于屋顶。
 
发明内容
为了解决上述技术问题,本发明提供了一种彩色涂层压花铝板。
一种彩色涂层压花铝板,其特征在于其通过包括如下步骤的方法制成:
1)将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油;
2)进入清洗槽内进行清洗;
3)清洗后进入钝化槽钝化,在钝化层上涂上底漆,然后进入烘箱烘干;
4)进入涂装线辊涂,再进入烘箱烘干;
5)经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。
所述的一种彩色涂层压花铝板,其特征在于步骤1)中的脱脂剂为铝酸脱,脱脂在常温条件下进行时间为1分钟。
所述的一种彩色涂层压花铝板,其特征在于步骤2)中清洗的温度为15—25℃,清洗时间为10秒,清洗槽的PH值控制在5—7。
所述的一种彩色涂层压花铝板,其特征在于步骤3)中钝化槽钝化在常温条件下进行,时间为10秒。
所述的一种彩色涂层压花铝板,其特征在于步骤3)中烘箱烘干的温度为80—120℃。
所述的一种彩色涂层压花铝板,其特征在于步骤4)中涂装线辊涂的是聚酯涂料或丙烯酸涂料。
所述的一种彩色涂层压花铝板,其特征在于步骤4)中烘箱的温度为250-270℃,烘干时间为60秒。
本发明的一种彩色涂层压花铝板,使得该产品抗紫外线和耐酸耐碱性能更强。同时,该产品既有彩钢的高强度性能,又有耐腐蚀、美观的优点,可用于屋顶。
附图说明
图1是本发明的生产工艺流程图。
 
具体实施方式
实施例1
彩色涂层压花铝板,通过包括如下步骤的方法制成:
1)将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油,脱脂剂为铝酸脱,脱脂在常温条件下进行时间为1分钟;
2)进入清洗槽内进行清洗,清洗的温度为15℃,清洗时间为10秒,清洗槽的PH值控制在5。
3)清洗后进入钝化槽钝化,钝化在常温条件下进行,时间为10秒,在钝化层上涂上底漆,然后进入烘箱烘干,烘干温度为80℃;
4)进入涂装线辊涂聚酯涂料,再进入烘箱烘干,烘箱的温度为250℃,烘干时间为60秒;
5)经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。
 
实施例2
彩色涂层压花铝板,通过包括如下步骤的方法制成:
1)将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油,脱脂剂为铝酸脱,脱脂在常温条件下进行时间为1分钟;
2)进入清洗槽内进行清洗,清洗的温度为20℃,清洗时间为10秒,清洗槽的PH值控制在6。
3)清洗后进入钝化槽钝化,钝化在常温条件下进行,时间为10秒,在钝化层上涂上底漆,然后进入烘箱烘干,烘干温度为100℃;
4)进入涂装线辊涂聚酯涂料,再进入烘箱烘干,烘箱的温度为260℃,烘干时间为60秒;
5)经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。
 
实施例3
彩色涂层压花铝板,通过包括如下步骤的方法制成:
1)将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油,脱脂剂为铝酸脱,脱脂在常温条件下进行时间为1分钟;
2)进入清洗槽内进行清洗,清洗的温度为25℃,清洗时间为10秒,清洗槽的PH值控制在7。
3)清洗后进入钝化槽钝化,钝化在常温条件下进行,时间为10秒,在钝化层上涂上底漆,然后进入烘箱烘干,烘干温度为120℃;
4)进入涂装线辊涂聚酯涂料,再进入烘箱烘干,烘箱的温度为270℃,烘干时间为60秒;
5)经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。
 
实施例2的产品经过检测,主要性能技术指标如下:
涂层厚度:≧18um;
铅笔硬度:≧2H(普通压花铝板为1H);
附着力:不次于1级;
柔韧性:≤2T(普通压花铝板为3T);
光泽度:光泽<70时,极限误差≤10%    光泽≧70时,极限误差≤5%;
色差:△E≤2(普通压花铝板△E≥3);
耐沸水性:2小时无变化(普通压花铝板1小时有变化)。
以上所述仅为本发明的较佳实施例,并不用以限制本发明,凡在本发明的精神和原则之内所作的任何修改、等同替换和改进等,均包含在本发明的保护范围之内。

Claims (7)

1.一种彩色涂层压花铝板,其特征在于其通过包括如下步骤的方法制成:
1)将铝板进行放卷,通过传动轴放入脱脂槽中进行脱脂除油;
2)进入清洗槽内进行清洗;
3)清洗后进入钝化槽钝化,在钝化层上涂上底漆,然后进入烘箱烘干;
4)进入涂装线辊涂,再进入烘箱烘干;
5)经过检验、收卷、放卷后放入压花线进行压花,最后收卷成品。
2.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤1)中的脱脂剂为铝酸脱,脱脂在常温条件下进行时间为1分钟。
3.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤2)中清洗的温度为15—25℃,清洗时间为10秒,清洗槽的PH值控制在5—7。
4.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤3)中钝化槽钝化在常温条件下进行,时间为10秒。
5.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤3)中烘箱烘干的温度为80—120℃。
6.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤4)中涂装线辊涂的是聚酯涂料或丙烯酸涂料。
7.如权利要求1所述的一种彩色涂层压花铝板,其特征在于步骤4)中烘箱的温度为250-270℃,烘干时间为60秒。
CN201410124792.3A 2014-03-31 2014-03-31 一种彩色涂层压花铝板 Expired - Fee Related CN103924744B (zh)