CN103067541A - 一种手机玻璃盖板的制作工艺 - Google Patents
一种手机玻璃盖板的制作工艺 Download PDFInfo
- Publication number
- CN103067541A CN103067541A CN2012105896098A CN201210589609A CN103067541A CN 103067541 A CN103067541 A CN 103067541A CN 2012105896098 A CN2012105896098 A CN 2012105896098A CN 201210589609 A CN201210589609 A CN 201210589609A CN 103067541 A CN103067541 A CN 103067541A
- Authority
- CN
- China
- Prior art keywords
- glass
- cover plate
- processed
- mobile phone
- cleaning
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明公开了一种手机玻璃盖板的制作工艺,包括以下步骤:(1)将原材玻璃清洗干净;(2)磨砂处理;(3)玻璃切割;(4)清洗;(5)精雕磨边仿形;(6)清洗;(7)化学钢化;(8)清洗;(9)丝网印刷;(10)烘干;(11)超声波清洗。本发明的一种手机玻璃盖板的制作工艺,通过该制作工艺得到的手机玻璃盖板表面层为磨砂层,当外界颗粒物在盖板表面移动时,磨砂层上具有的颗粒能有效阻碍外界颗粒物对盖板表面的伤害,防止盖板表面被划花;同时在强光的入射后,盖板磨砂层会产生多种漫反射抵消整体图案的反射,减小盖板的反射性,从而提高了产品的实用性,满足人们需要,节约使用成本。
Description
技术领域
本发明涉及一种手机玻璃盖板生产工艺,具体涉及一种手机玻璃盖板的制作工艺。
背景技术
随着无线通讯技术的迅猛发展,手机已越来越普遍地进入百姓生活中,手机用户也逐年快速增长。同时,手机的更新换代及淘汰速度也在变快。其中,手机淘汰的原因之一是因为手机光洁屏幕被刮花,变得模糊,且光洁手机屏幕镜面在强光入射下会产生反射,反射光让手机使用者难以看清楚手机显示屏上的内容。于是,有人提出了一些对手机屏幕起保护作用的装置,比如贴手机膜,但由于其制造工艺复杂或成本高昂或安装后使用不方便或更换频率高等缺陷,一直无法满足人们的需要。
发明内容
针对上述存在的技术问题,本发明的目的是:提出了一种能够提高手机玻璃盖板的抗划伤性以及减小手机玻璃盖板的光反射性的手机玻璃盖板的制作工艺。
本发明的技术解决方案是这样实现的:一种手机玻璃盖板的制作工艺,包括以下步骤:
(1)将原材玻璃清洗干净:选取原材质的白玻璃,对其清洗干净;
(2)磨砂处理:采用表面喷砂工艺将将经步骤(1)处理后的玻璃进行表面磨砂处理;
(3)玻璃切割:将经步骤(2)处理后的玻璃切割成所需的外观大小;
(4)清洗:将经步骤(3)处理后的玻璃进行清洗干净;
(5)精雕磨边仿形:利用数控机床对经步骤(4)处理的玻璃进行精雕、磨边仿形操作,使得磨砂玻璃的每个边缘的切面磨成磨砂面;
(6)清洗:将经步骤(5)处理后的磨砂玻璃进行超声波清洗;
(7)化学钢化:将经步骤(6)处理后的玻璃进行化学钢化处理;
(8)清洗:将经步骤(7)处理后的磨砂玻璃进行超声波清洗;
(9)丝网印刷:采用丝网印刷机将油墨印刷在经步骤(8)处理后的玻璃四周边处;
(10)烘干:将经步骤(9)处理后的玻璃置于烘干机中进行烘干后成型;
(11)清洗:将经步骤(10)成型产品进行超声波清洗。
由于上述技术方案的运用,本发明与现有技术相比具有下列优点:
本发明的一种手机玻璃盖板的制作工艺,通过该制作工艺得到的手机玻璃盖板表面层为磨砂层,当外界颗粒物在盖板表面移动时,磨砂层上具有的颗粒能有效阻碍外界颗粒物对盖板表面的伤害,防止盖板表面被划花;同时在强光的入射后,盖板磨砂层会产生多种漫反射抵消整体图案的反射,减小盖板的反射性,从而提高了产品的实用性,满足人们需要,节约使用成本。
附图说明
下面结合附图对本发明技术方案作进一步说明:
附图1为本发明的手机玻璃盖板的制作工艺的工艺方法流程图。
具体实施方式
下面结合附图来说明本发明。
如附图1所示为本发明所述的一种手机玻璃盖板的制作工艺,包括以下步骤:
第一步,将原材玻璃清洗干净:选取原材质的白玻璃,对其清洗干净,得到原材玻璃A;
第二步,磨砂处理:采用表面喷砂工艺将将经步骤一处理后的原材玻璃A进行表面磨砂处理,得到磨砂玻璃B;
第三步,玻璃切割:将经步骤二处理后的磨砂玻璃B切割成所需外观大小的手机玻璃盖板C;
第四步,清洗:将经步骤三处理后的手机玻璃盖板C进行清洗干净;
第五步,精雕磨边仿形:利用数控机床对经步骤四清洗后的手机玻璃盖板C进行精雕、磨边仿形操作,使得玻璃盖板C的每个边缘的切面磨成磨砂面,得到手机玻璃盖板D;
第六步,超声波清洗:将经步骤五处理后的手机玻璃盖板D进行超声波清洗;
第七步,化学钢化:将经步骤六清洗后的玻璃盖板D进行化学钢化处理,得到手机玻璃盖板E;
第八步,清洗:将经步骤七处理后的玻璃盖板E进行超声波清洗;
第九步,丝网印刷:采用丝网印刷机将油墨印刷在经步骤八清洗后的玻璃盖板E四周边处,得到手机玻璃盖板F;
第十步,烘干:将经步骤九处理后的手机玻璃盖板F置于烘干机中进行烘干后成型;
第十一步,清洗:将经步骤十烘干成型产品进行超声波清洗。
上述实施例只为说明本发明的技术构思及特点,其目的在于让熟悉此项技术的人士能够了解本发明的内容并加以实施,并不能以此限制本发明的保护范围,凡根据本发明精神实质所作的等效变化或修饰,都应涵盖在本发明的保护范围内。
Claims (1)
1.一种手机玻璃盖板的制作工艺,其特征在于,包括以下步骤:
(1)将原材玻璃清洗干净:选取原材质的白玻璃,对其清洗干净;
(2)磨砂处理:采用表面喷砂工艺将将经步骤(1)处理后的玻璃进行表面磨砂处理;
(3)玻璃切割:将经步骤(2)处理后的玻璃切割成所需的外观大小;
(4)清洗:将经步骤(3)处理后的玻璃进行清洗干净;
(5)精雕磨边仿形:利用数控机床对经步骤(4)处理的玻璃进行精雕、磨边仿形操作,使得磨砂玻璃的每个边缘的切面磨成磨砂面;
(6)清洗:将经步骤(5)处理后的磨砂玻璃进行超声波清洗;
(7)化学钢化:将经步骤(6)处理后的玻璃进行化学钢化处理;
(8)清洗:将经步骤(7)处理后的磨砂玻璃进行超声波清洗;
(9)丝网印刷:采用丝网印刷机将油墨印刷在经步骤(8)处理后的玻璃四周边处;
(10)烘干:将经步骤(9)处理后的玻璃置于烘干机中进行烘干后成型;
(11)清洗:将经步骤(10)成型产品进行超声波清洗。