CN102294322A - 一种油漆钢琴漆面的方法 - Google Patents

一种油漆钢琴漆面的方法 Download PDF

Info

Publication number
CN102294322A
CN102294322A CN2011102331274A CN201110233127A CN102294322A CN 102294322 A CN102294322 A CN 102294322A CN 2011102331274 A CN2011102331274 A CN 2011102331274A CN 201110233127 A CN201110233127 A CN 201110233127A CN 102294322 A CN102294322 A CN 102294322A
Authority
CN
China
Prior art keywords
polishing
paint
lacquer
piano
wood
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2011102331274A
Other languages
English (en)
Inventor
何志雄
余成强
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHONGSHAN FOURSEAS FURNITURE Manufacturing Co Ltd
Original Assignee
ZHONGSHAN FOURSEAS FURNITURE Manufacturing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHONGSHAN FOURSEAS FURNITURE Manufacturing Co Ltd filed Critical ZHONGSHAN FOURSEAS FURNITURE Manufacturing Co Ltd
Priority to CN2011102331274A priority Critical patent/CN102294322A/zh
Publication of CN102294322A publication Critical patent/CN102294322A/zh
Pending legal-status Critical Current

Abstract

本发明涉及家具制造领域,具体公开一种油漆钢琴漆面的方法,依次包括:一次打磨步骤,在木材表面打磨,处理木材表面瑕疵;塑色步骤,在打磨后的木材表面直接喷涂塑色油,对木材表面塑色;喷涂底面漆步骤,对塑色后的木材表面喷涂底面两用漆,形成一底面漆层;二次打磨步骤,对底面漆层进行二次打磨,处理底面漆层表面的瑕疵;抛光步骤,对打磨后的底面漆层进行抛光,得到钢琴漆面。本发明可简化油漆钢琴漆面的工艺补助,提高钢琴漆面的效果。

Description

一种油漆钢琴漆面的方法
技术领域
本发明涉及家具制造领域,特别涉及一种油漆钢琴漆面方法。
背景技术
目前,对家具的制作工艺要求越来越高,其中油漆工艺是其中的关键。为了提高家具的外观效果,在高档家具中常使用钢琴漆工艺,它是烤漆工艺的一种,工序非常复杂:首先,需要在木板上涂以腻子,作为喷漆的底层;将腻子找平后待腻子干透,进行抛光打磨光滑;然后反复喷涂3-5次底漆,每次喷涂后,都要用水砂纸和磨布抛光;最后,再喷涂1-3次亮光型的面漆,然后使用高温烘烤,使漆层固化;最终实现较好的漆面效果。
申请人已采用一种油漆钢琴漆面的工艺,在常用家具表面油漆处理工艺的流程是:打磨→喷底漆→打磨→修色→喷面漆。该工艺方案相对于烤漆工艺更为简单,但也存在油漆透明性、明亮性较差,塑色效果、素材木皮纹理显示不够清晰的缺陷,其原因在于以下原因:一方面,工艺方案所用油漆的透明度低;另一方面,分开底漆及面漆喷涂,木材表面履盖了两层油漆,同样影响了漆面透明度。
发明内容
有鉴于此,本发明的目的在于提供一种油漆钢琴漆面的方法,可简化工艺,提高漆面效果。
为解决以上技术问题,本发明提供的技术方案是,一种油漆钢琴漆面的方法,依次包括:
一次打磨步骤,在木材表面打磨,处理木材表面瑕疵;
塑色步骤,在打磨后的木材表面直接喷涂塑色油,对木材表面塑色;
喷涂底面漆步骤,对塑色后的木材表面喷涂底面两用漆,形成一底面漆层;
二次打磨步骤,对底面漆层进行二次打磨,处理底面漆层表面的瑕疵;
抛光步骤,对打磨后的底面漆层进行抛光,得到钢琴漆面。
较优地,所述二次打磨步骤与所述抛光步骤之间包括水磨步骤,对底面漆表面打水磨处理,去除漆面瑕疵。
较优地,所述水磨步骤中,先后采用分别是800#水砂纸和1500#水砂纸进行水磨。
较优地,所述喷涂底面漆步骤中,喷涂底面两用漆的厚度至1mm-2mm。
较优地,喷涂涂底面两用漆过程中,间隔3~4次停顿,每次停顿10~20分钟。
较优地,所述一次打磨步骤中,顺木纹方向打磨木材表面。
较优地,所述二次打磨步骤中,顺木纹方向打磨底面漆层。
较优地,所述抛光步骤中,先后用粗蜡和幼蜡进行抛光。
较优地,所述底面两用漆为PE全透明底面两用漆。
与现有技术相比,本发明的油漆用料及工艺制作方法都明显的差异:主材采用底面两用漆,最大特点是底漆与面漆可以合用,因而可仅喷涂一次,有助于简化工艺;特殊的打磨、抛光工序使得油漆钢琴漆面,亮光、全透明,木材表面颜色、纹理清晰。
附图说明
图1是本发明油漆钢琴漆面的方法一优选实施例的流程图。
具体实施方式
本发明优选实施例的关键在于:1、油漆一次性厚涂;2、油漆表面打水磨,再抛光处理。
为了使本领域的技术人员更好地理解本发明的技术方案,下面结合附图和具体实施例对本发明作进一步的详细说明。
参见图1,表示本发明油漆钢琴漆面的方法一优选实施例。该油漆钢琴漆面方法的具体工艺流程为:
S101、在木材表面打磨,处理木材表面瑕疵。
一次打磨步骤中,通过木材表面打磨,处理木材表面瑕疵,包括洞眼、拼缝、胶水印痕等,需保证手感光滑。其技术要点为顺木纹方向打磨,这是因为:沿木材纹理打磨,砂纸的砂痕会与木材纹理同一方向,使砂痕不明显;假若与木材纹理方向交叉打磨,砂痕将会非常明显。
S102、塑色步骤,在打磨后的木材表面直接喷涂塑色油,对木材表面塑色。
塑色步骤中,木材表面塑色采用喷涂技术直接在木材表面塑色,使木材表面颜色更加鲜明、清晰。其技术要点为:修色过程中应掌握油量大小及油枪行走速度的均匀性,相关参数和数值范围具体可根据操作需要确定。
S103、对塑色后的木材表面喷涂底面两用漆,形成一底面漆层。
该喷涂底面漆步骤中,木材表面只需一次性喷涂底面漆(优选为PE全透明底面两用漆,如型号为T20029S),使油漆厚度喷涂至1mm-2mm之间。这是因为:底面漆为底漆与面漆共用的油漆,故只须喷涂一次,而无需将底漆与面漆分开喷涂,这也是本发明较现有技术的重要区别点。该步骤的技术难点是:油漆喷涂过厚,容易引起流油、油漆发白等。解决方法是:每次厚涂,中间隔3~4次停顿,每次停顿10~20分钟。
S104、对底面漆层进行二次打磨,处理底面漆层表面的瑕疵。
此二次打磨步骤中,将油漆表面打磨,处理油漆表面瑕疵,包括洞眼、流油、橘皮、窝点,漆面不平等,为下一步抛光作准备。该步骤的技术要点为:根据油漆表面的粗糙程度控制下压力度(相关的参数范围具体可根据操作需要确定),顺木纹方向打磨。
S105、对底面漆表面打水磨处理,去除漆面瑕疵。
此水磨步骤为优选步骤,其先后采用分别是800#水砂纸和1500#水砂纸进行水磨对底面漆表面打水磨处理,去除漆面的一切瑕疵。
S106、对打磨后的底面漆层进行抛光,得到钢琴漆面。
该步骤中先后用粗、幼蜡抛光水磨处理后的油漆表面,直至漆面达到明亮的镜面效果。当然,步骤S105、S106也可视为同一步骤的两个阶段,不再赘述。
本发明油漆主材采用底面两用漆,其最大特点是底漆与面漆可以合用,因而可仅喷涂一次,简化了工艺;而特殊的打磨、抛光工序使得油漆钢琴漆面,亮光、全透明,木材表面颜色、纹理清晰。
以上仅是本发明的优选实施方式,应当指出的是,上述优选实施方式不应视为对本发明的限制,本发明的保护范围应当以权利要求所限定的范围为准。对于本技术领域的普通技术人员来说,在不脱离本发明的精神和范围内,还可以做出若干改进和润饰,这些改进和润饰也应视为本发明的保护范围。

Claims (9)

1.一种油漆钢琴漆面的方法,其特征在于,依次包括:
一次打磨步骤,在木材表面打磨,处理木材表面瑕疵;
塑色步骤,在打磨后的木材表面直接喷涂塑色油,对木材表面塑色;
喷涂底面漆步骤,对塑色后的木材表面喷涂底面两用漆,形成一底面漆层;
二次打磨步骤,对底面漆层进行二次打磨,处理底面漆层表面的瑕疵;
抛光步骤,对打磨后的底面漆层进行抛光,得到钢琴漆面。
2.如权利要求1所述的油漆钢琴漆面的方法,其特征在于,所述二次打磨步骤与所述抛光步骤之间包括水磨步骤,对底面漆表面打水磨处理,去除漆面瑕疵。
3.如权利要求2所述的油漆钢琴漆面的方法,其特征在于,所述水磨步骤中,先后采用分别是800#水砂纸和1500#水砂纸进行水磨。
4.如权利要求1所述油漆钢琴漆面的方法,其特征在于,所述喷涂底面漆步骤中,喷涂底面两用漆的厚度至1mm-2mm。
5.如权利要求4所述油漆钢琴漆面的方法,其特征在于,喷涂涂底面两用漆过程中,间隔3~4次停顿,每次停顿10~20分钟。
6.如权利要求1所述油漆钢琴漆面的方法,其特征在于,所述一次打磨步骤中,顺木纹方向打磨木材表面。
7.如权利要求1所述油漆钢琴漆面的方法,其特征在于,所述二次打磨步骤中,顺木纹方向打磨底面漆层。
8.如权利要求1所述油漆钢琴漆面的方法,其特征在于,所述抛光步骤中,先后用粗蜡和幼蜡进行抛光。
9.如权利要求1~8任一项所述油漆钢琴漆面的方法,其特征在于,所述底面两用漆为PE全透明底面两用漆。
CN2011102331274A 2011-08-15 2011-08-15 一种油漆钢琴漆面的方法 Pending CN102294322A (zh)