WO2026028601A1 - 架橋ゴム組成物及びそれを用いた伝動ベルト - Google Patents
架橋ゴム組成物及びそれを用いた伝動ベルトInfo
- Publication number
- WO2026028601A1 WO2026028601A1 PCT/JP2025/020496 JP2025020496W WO2026028601A1 WO 2026028601 A1 WO2026028601 A1 WO 2026028601A1 JP 2025020496 W JP2025020496 W JP 2025020496W WO 2026028601 A1 WO2026028601 A1 WO 2026028601A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- rubber composition
- mass
- rubber
- content
- component
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L23/00—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers
- C08L23/02—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers not modified by chemical after-treatment
- C08L23/04—Homopolymers or copolymers of ethene
- C08L23/08—Copolymers of ethene
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L23/00—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers
- C08L23/02—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers not modified by chemical after-treatment
- C08L23/16—Ethylene-propylene or ethylene-propylene-diene copolymers
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L57/00—Compositions of unspecified polymers obtained by reactions only involving carbon-to-carbon unsaturated bonds
- C08L57/02—Copolymers of mineral oil hydrocarbons
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L61/00—Compositions of condensation polymers of aldehydes or ketones; Compositions of derivatives of such polymers
- C08L61/04—Condensation polymers of aldehydes or ketones with phenols only
- C08L61/06—Condensation polymers of aldehydes or ketones with phenols only of aldehydes with phenols
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16G—BELTS, CABLES, OR ROPES, PREDOMINANTLY USED FOR DRIVING PURPOSES; CHAINS; FITTINGS PREDOMINANTLY USED THEREFOR
- F16G1/00—Driving-belts
- F16G1/06—Driving-belts made of rubber
Definitions
- the present invention relates to a crosslinked rubber composition and a transmission belt using the same.
- Ethylene- ⁇ -olefin elastomers are widely used as the rubber component of cross-linked rubber compositions used to form rubber products.
- Patent Documents 1 to 3 disclose the use of a blend rubber of ethylene propylene diene terpolymer and ethylene-1-butenediene terpolymer as the rubber component of a cross-linked rubber composition for transmission belts.
- Patent No. 7458859 Patent No. 7458860
- the present invention relates to a crosslinked rubber composition obtained by crosslinking an uncrosslinked rubber composition.
- the uncrosslinked rubber composition contains a first rubber component that is an ethylene- ⁇ -olefin elastomer in which the ⁇ -olefin is propylene, a second rubber component that is an ethylene-1-butenediene terpolymer, and a tackifier.
- the present invention is a power transmission belt formed at least in part from the crosslinked rubber composition of the present invention.
- FIG. 1 A first figure.
- the cross-linked rubber composition X according to this embodiment is obtained by cross-linking the uncross-linked rubber composition X'.
- the uncross-linked rubber composition X' contains a first rubber component that is an ethylene- ⁇ -olefin elastomer in which the ⁇ -olefin is propylene, a second rubber component that is an ethylene-1-butenediene terpolymer (EBDM), and a tackifier.
- EBDM ethylene-1-butenediene terpolymer
- crosslinked rubber compositions containing ethylene propylene diene terpolymer or ethylene propylene copolymer as the rubber component have low adhesiveness before crosslinking. Therefore, when using the uncrosslinked rubber composition to form an uncrosslinked molded article, for example, when laminating a sheet-shaped uncrosslinked rubber composition or when compounding the uncrosslinked rubber composition with a fibrous material, the poor adhesion of the uncrosslinked rubber composition results in poor molding processability.
- the uncrosslinked rubber composition X' before crosslinking contains a first rubber component of an ethylene- ⁇ -olefin elastomer in which the ⁇ -olefin is propylene, a second rubber component of EBDM, and a tackifier, thereby enabling the uncrosslinked rubber composition X' before crosslinking to achieve excellent molding processability.
- a first rubber component of an ethylene- ⁇ -olefin elastomer in which the ⁇ -olefin is propylene a second rubber component of EBDM, and a tackifier
- the first rubber component contains ethylene propylene diene terpolymer (EPDM) and/or ethylene propylene copolymer (EPR). Therefore, the first rubber component may be composed of EPDM alone, EPR alone, or a blend rubber of EPDM and EPR. From the viewpoint of obtaining excellent molding processability from the uncrosslinked rubber composition X' before crosslinking, it is preferable that the first rubber component contain EPDM.
- EPDM ethylene propylene diene terpolymer
- EPR ethylene propylene copolymer
- the diene component examples include 5-ethylidene-2-nobornene (ENB), 5-vinyl-2-nobornene (VNB), dicyclopentadiene, and 1,4-hexadiene.
- ENB is preferred as the diene component from the viewpoint of obtaining excellent moldability of the uncrosslinked rubber composition X' before crosslinking.
- the ENB content (diene content) of the EPDM contained in the first rubber component is preferably 4% by mass or more and 12% by mass or less, more preferably 6% by mass or more and 10% by mass or less, and even more preferably 7.5% by mass or more and 8.5% by mass or less, from the same viewpoints as above.
- the ethylene content of the EBDM of the second rubber component is preferably 40% by mass or more and 60% by mass or less, more preferably 45% by mass or more and 55% by mass or less, and even more preferably 48% by mass or more and 52% by mass or less.
- the ratio of the ethylene content of the second rubber component to the ethylene content of the first rubber component is preferably 0.7 or more and 1 or less, more preferably 0.85 or more and less than 1, even more preferably 0.9 or more and 0.99 or less, still more preferably 0.93 or more and 0.98 or less, and even more preferably 0.95 or more and 0.97 or less.
- diene components of the second rubber component examples include ENB, VNB, dicyclopentadiene, and 1,4-hexadiene.
- ENB is preferred as the diene component from the viewpoint of obtaining excellent moldability of the uncrosslinked rubber composition X' before crosslinking.
- the ENB content (diene content) of the EBDM of the second rubber component is preferably 4% by mass or more and 10% by mass or less, more preferably 6% by mass or more and 8% by mass or less, and even more preferably 6.5% by mass or more and 7.5% by mass or less.
- the difference between the ENB content of the EBDM of the second rubber component and the ENB content of the EPDM contained in the first rubber component is small, from the viewpoint of homogenizing the crosslinked rubber composition X after crosslinking.
- the difference between the ENB content of the EPDM contained in the first rubber component and the ENB content of the EBDM of the second rubber component is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and even more preferably 1.5% by mass or less.
- the ENB content of the EBDM of the second rubber component is the same as or less than the ENB content of the EPDM contained in the first rubber component.
- the ratio of the ENB content of the EBDM of the second rubber component to the ENB content of the EPDM contained in the first rubber component is preferably 0.4 or more and 1 or less, more preferably 0.6 or more and less than 1, even more preferably 0.8 or more and 0.95 or less, still more preferably 0.83 or more and 0.93 or less, and even more preferably 0.85 or more and 0.9 or less.
- the content A1 of the first rubber component in the uncrosslinked rubber composition X' may be greater than, less than, or the same as the content A2 of the second rubber component, but from the viewpoint of obtaining excellent moldability of the uncrosslinked rubber composition X' before crosslinking, it is preferable that the content A1 of the first rubber component be equal to or greater than A2.
- the mass ratio (A1/A2) of the content A1 of the first rubber component to the content A2 of the second rubber component is preferably 50/50 or greater and 90/10 or less, 55/45 or greater and 80/20 or less, or 60/40 or greater and 70/30 or less.
- Uncrosslinked rubber composition X' may contain a rubber component other than the first and second rubber components in an amount less than the total amount of the first and second rubber components.
- rubber components other than the first and second rubber components include ethylene-1-butene copolymer (EBR), chloroprene rubber (CR), and hydrogenated nitrile rubber (H-NBR).
- tackifiers include phenolic resin-based tackifiers, petroleum resin-based tackifiers, rosin resin-based tackifiers, terpene resin-based tackifiers, and coumarone-indene resin-based tackifiers.
- phenolic resin-based tackifiers include alkylphenol resins, alkylphenol-formaldehyde resins, and phenol-formaldehyde resins.
- Examples of petroleum resin-based tackifiers include C5-C9 petroleum resins made from C5 and C9 fractions, C5 petroleum resins made from C5 fractions, C9 petroleum resins made from C9 fractions, and dicyclopentadiene petroleum resins.
- Examples of rosin resin-based tackifiers include rosin ester resins and hydrogenated rosin ester resins.
- Examples of terpene resin-based tackifiers include polyterpene resins and styrene-modified terpene resins.
- Examples of coumarone-indene resin-based tackifiers include coumarone-indene resins and hydrogenated coumarone-indene resins. The tackifier preferably contains one or more of these.
- a phenolic resin-based tackifier and/or a petroleum resin-based tackifier and more preferably an alkylphenol resin and/or a C5-C9 petroleum resin.
- alkylphenol resin tackifiers include, for example, Tamanol (registered trademark) 100S, 200N, 510, 521, 526, 586, and 7509 manufactured by Arakawa Chemical Industries, Ltd.
- C5-C9 petroleum resin tackifiers include, for example, Petrotack (registered trademark) 60, 70, 90, 90V, 90HS, and 100V manufactured by Tosoh Corporation.
- the tackifier content B in uncrosslinked rubber composition X' is preferably 1 part by mass or more and 10 parts by mass or less, more preferably 2 parts by mass or more and 7 parts by mass or less, and even more preferably 3 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the total content of the first and second rubber components.
- the mass ratio (B/A2) of the tackifier content B in uncrosslinked rubber composition X' to the second rubber component content A2 is preferably 0.04 or more and 0.8 or less, more preferably 0.05 or more and 0.2 or less, and even more preferably 0.06 or more and 0.15 or less.
- the softening point of the tackifier is preferably 70°C or higher and 100°C or lower, from the viewpoint of obtaining excellent moldability of the uncrosslinked rubber composition X' before crosslinking while suppressing a decrease in hardness of the crosslinked rubber composition X after crosslinking. This softening point is measured by the ring and ball method.
- the uncrosslinked rubber composition X' preferably contains a crosslinking agent for thermally crosslinking the first and second rubber components.
- crosslinking agents include sulfur and organic peroxides.
- organic peroxides include ⁇ , ⁇ '-di(t-butylperoxy)diisopropylbenzene, dicumyl peroxide, 1,3-bis(t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.
- the organic peroxide preferably contains one or more of these, and more preferably contains ⁇ , ⁇ '-di(t-butylperoxy)diisopropylbenzene.
- the crosslinking agent may contain either sulfur or an organic peroxide, or both sulfur and an organic peroxide.
- the amount of sulfur in the uncrosslinked rubber composition X' is, for example, 2 to 4 parts by mass per 100 parts by mass of the combined content of the first and second rubber components.
- the amount of organic peroxide blended in uncrosslinked rubber composition X' is, for example, 2.5 parts by mass or more and 3.5 parts by mass or less per 100 parts by mass of the total content of the first and second rubber components.
- Uncrosslinked rubber composition X' may also contain, as necessary, reinforcing materials such as carbon black, silica, and short fibers, co-crosslinking agents, process oils, plasticizers, processing aids, vulcanization accelerators, vulcanization accelerators, antioxidants, etc.
- reinforcing materials such as carbon black, silica, and short fibers, co-crosslinking agents, process oils, plasticizers, processing aids, vulcanization accelerators, vulcanization accelerators, antioxidants, etc.
- the cross-linked rubber composition X according to this embodiment can be suitably used to form, for example, at least a portion of a transmission belt.
- the rubber belt body 10 is composed of an adhesive rubber layer 101 in which the core wires 11 are embedded, an inner compression rubber layer 102 whose inner surface is covered with reinforcing cloth 12, and an outer tension rubber layer 103 whose outer surface is covered with reinforcing cloth 13. Any one, two, or all three layers of the adhesive rubber layer 101, compression rubber layer 102, and tension rubber layer 103 can be formed from the crosslinked rubber composition X of the embodiment.
- the rubber belt body 20 is composed of a back rubber portion 201 in which the core wires 21 are embedded and a tooth rubber portion 202 covered with reinforcing cloth 22.
- One or both of the back rubber portion 201 and the tooth rubber portion 202 can be formed from the crosslinked rubber composition X.
- the cords 11, 21 are provided with adhesive layers for bonding to the belt bodies 10, 20, and these adhesive layers can be formed from crosslinked rubber composition X.
- the reinforcing fabrics 12, 13, 22 are provided with internally impregnated adhesive portions and/or inner adhesive layers for bonding to the belt bodies 10, 20, and these internally impregnated adhesive portions and/or inner adhesive layers can be formed from crosslinked rubber composition X.
- the manufacturing method of these V-belts B and toothed belts C may include a step of laminating sheet-shaped uncrosslinked rubber composition X' and/or a step of compounding the uncrosslinked rubber composition X' with a fiber member core wire 11, 21 or a reinforcing cloth 12, 13, 22, and a step of producing a cylindrical belt slab by heating and pressurizing the uncrosslinked slab to crosslink the uncrosslinked rubber composition X' and form a crosslinked rubber composition X.
- the process of molding a cylindrical uncrosslinked slab includes a step of laminating sheet-like uncrosslinked rubber composition X' and/or a step of compounding uncrosslinked rubber composition X' with the cords 11, 21 of the fiber member and the reinforcing fabrics 12, 13, 22. Because the adhesiveness of uncrosslinked rubber composition X' is increased, high adhesion between sheets of uncrosslinked rubber composition X' and/or high adhesion of uncrosslinked rubber composition X' to the cords 11, 21 and the reinforcing fabrics 12, 13, 22 is obtained, and excellent molding processability due to uncrosslinked rubber composition X' can be obtained when molding the uncrosslinked slab.
- the manufacturing method for V-belt B or toothed belt C may include a step of immersing the core wires 11, 21 in a rubber cement prepared by dissolving uncrosslinked rubber composition X' in an organic solvent, followed by heating to perform an adhesive treatment, thereby coating the outer periphery of the core wires 11, 21 with an overcoat layer of uncrosslinked rubber composition X'.
- the overcoat layer is formed in the adhesive layer at the interface between the core wires 11, 21 and the belt body 10, 20 when the uncrosslinked slab is heated and pressurized.
- the overcoat layer of uncrosslinked rubber composition X' provides high adhesiveness to the core wires 11, 21, and therefore the overcoat layer of uncrosslinked rubber composition X' provides excellent molding processability when molding the uncrosslinked slab.
- the soaking layer is formed in the internal impregnated adhesive portion that covers the yarn surfaces inside the reinforcing fabrics 12, 13, and 22 when the uncrosslinked slab is heated and pressurized.
- the coating layer is formed on the inner adhesive layer of the reinforcing fabrics 12, 13, 22 at the interface with the belt main body 10, 20 when the uncrosslinked slab is heated and pressurized.
- the soaking layer and/or coating layer of uncrosslinked rubber composition X' provides high adhesion to the reinforcing fabrics 12, 13, 22, thereby achieving excellent molding processability when molding the uncrosslinked slab due to the soaking layer and/or coating layer of uncrosslinked rubber composition X'.
- EPDM1 EP33 manufactured by ENEOS Materials Corporation, ethylene content: 52 mass%, ENB content: 8.1 mass%)
- EBDM K-9330M manufactured by Mitsui Chemicals, Inc., ethylene content: 50 mass%, ENB content: 7.1 mass%)
- the kneading temperature was set to a temperature higher than the softening point of the tackifier.
- the difference between the ethylene content of the first rubber component and the ethylene content of the second rubber component is 2% by mass.
- the content ratio of the ethylene content of the second rubber component to the ethylene content of the first rubber component is 0.96.
- the difference between the ENB content of the EPDM of the first rubber component and the ENB content of the EBDM of the second rubber component is 1% by mass.
- the content ratio of the ENB content of the EBDM of the second rubber component to the ENB content of the EPDM of the first rubber component is 0.88.
- This blend rubber of the first and second rubber components was mixed with 4 parts by mass of alkylphenol resin as a tackifier, 3 parts by mass of sulfur as a crosslinking agent (oil sulfur, manufactured by Hosoi Chemical Industry Co., Ltd.), 50 parts by mass of HAF carbon black, 20 parts by mass of silica, 5 parts by mass of process oil, 1 part by mass of stearic acid as a processing aid, 5 parts by mass of zinc oxide as a vulcanization accelerator aid, and 3 parts by mass of a vulcanization accelerator, per 100 parts by mass of the rubber component, and kneaded in a kneader to prepare an uncrosslinked rubber composition, designated Q1.
- the kneading temperature was set to a temperature higher than the softening point of the tackifier.
- EPDM1 Using EPDM1 as the rubber component, 100 parts by mass of the rubber component was blended with 4 parts by mass of alkylphenol resin as a tackifier, 7 parts by mass (2.8 parts by mass of active ingredient) of organic peroxide ⁇ , ⁇ '-di(t-butylperoxy)diisopropylbenzene (Peroximon F-40, manufactured by NOF Corporation, purity: 40%) as a crosslinking agent, 60 parts by mass of HAF carbon black, 15 parts by mass of aramid short fiber, 1.5 parts by mass of co-crosslinking agent, 5 parts by mass of process oil, 0.25 parts by mass of stearic acid as a processing aid, 5 parts by mass of zinc oxide as a vulcanization accelerator aid, and 2.5 parts by mass of an antioxidant, and kneaded in a kneader to prepare an uncrosslinked rubber composition, designated R.
- R uncrosslinked rubber composition
- Each of the uncrosslinked rubber compositions Q1 to Q4 for the overcoat layer was dissolved in an organic solvent to prepare a rubber paste.
- a core wire made of RFL-treated polyester fiber was immersed in each rubber paste, then removed and heated to dry, thereby coating the core wire with an overcoat layer of Q1 to Q4.
- the core wire coated with the overcoat layer was cut into several short pieces, which were then adhered in parallel to a rectangular sheet substrate to create test specimens for the tackiness test.
- the tackiness test was carried out using a pickup-type tack meter (Tack Tester IMC-1567, manufactured by Imoto Machinery Co., Ltd.).
- the tack meter has a cylindrical aluminum adhesive disc with a diameter of 50 mm and a thickness of 14 mm, with its axis extending horizontally from front to back, and a fixing plate below it for setting the test piece.
- the adhesive disc has its upper end connected to a load cell and is movable up and down together with the load cell.
- the specific test method is as follows.
- test piece was attached to the outer periphery of the adhesive disc on the fixed plate side with double-sided tape, and the other test piece was attached horizontally to the fixed plate with double-sided tape.
- the adhesive disc was lowered at a rate of 30 mm/min so as to approach the fixed plate, and one test piece was pressed against the other test piece with a load of 4.9 N. After 10 seconds, the adhesive disc was raised at a rate of 30 mm/min so as to separate it from the fixed plate.
- the peel force (tack force) when one test piece was peeled from the other test piece was then measured with a load cell.
- Test 1 the test piece on the disk side of the adhesive bond was designated P1.
- the peel force was measured for each of the test pieces on the fixed plate side: Example 1, Q2; Example 2, Q3; and Example 3, R.
- Test 2 the test piece on the disk side of the adhesive bond was designated P2. Peel strength was measured for Example 4, in which the test piece on the fixed plate side was designated Q2, Example 5, in which it was designated Q3, and Example 6, in which it was designated R.
- Test 3 the test piece on the disk side of the adhesive bond was designated P3.
- the peel force was measured for Example 7, in which the test piece on the fixed plate side was designated Q2, Comparative Example 1, in which it was designated Q3, and Comparative Example 2, in which it was designated R.
- Test 4 the test piece on the adhesive disk side was designated P4.
- the peel force was measured for each of the test pieces on the fixed portion side: Example 8 designated Q1, Example 9 designated Q2, Comparative Example 3 designated Q3, Comparative Example 4 designated Q4, and Comparative Example 5 designated R.
- Table 4 shows the test results for tests 1 to 4 when the test pieces on the adhesive disk side were P1 to P4, respectively.
- Table 5 shows the test results when the test pieces on the fixed part side were Q1 to Q4 and R, respectively.
- the present invention is useful in the technical fields of crosslinked rubber compositions and power transmission belts using the same.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Engineering & Computer Science (AREA)
- General Engineering & Computer Science (AREA)
- Oil, Petroleum & Natural Gas (AREA)
- Mechanical Engineering (AREA)
- Compositions Of Macromolecular Compounds (AREA)
- Adhesives Or Adhesive Processes (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2025533435A JPWO2026028601A1 (cg-RX-API-DMAC7.html) | 2024-07-30 | 2025-06-06 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2024-123263 | 2024-07-30 | ||
| JP2024123263 | 2024-07-30 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2026028601A1 true WO2026028601A1 (ja) | 2026-02-05 |
Family
ID=98606535
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2025/020496 Pending WO2026028601A1 (ja) | 2024-07-30 | 2025-06-06 | 架橋ゴム組成物及びそれを用いた伝動ベルト |
Country Status (2)
| Country | Link |
|---|---|
| JP (1) | JPWO2026028601A1 (cg-RX-API-DMAC7.html) |
| WO (1) | WO2026028601A1 (cg-RX-API-DMAC7.html) |
Citations (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2006138355A (ja) * | 2004-11-10 | 2006-06-01 | Bando Chem Ind Ltd | 伝動ベルト |
| JP2009137272A (ja) * | 2007-11-16 | 2009-06-25 | Toyoda Gosei Co Ltd | ウォーターホース及びホース用混合物 |
| WO2015122415A1 (ja) * | 2014-02-13 | 2015-08-20 | 三井化学株式会社 | エチレン・α-オレフィン・非共役ポリエン共重合体およびその用途、並びにその製造方法 |
| WO2021006018A1 (ja) * | 2019-07-08 | 2021-01-14 | Nok株式会社 | トーショナルダンパ用ゴム組成物 |
| JP2021080440A (ja) * | 2019-11-20 | 2021-05-27 | 三ツ星ベルト株式会社 | 成形用部材およびその用途 |
| JP2021161345A (ja) * | 2020-04-02 | 2021-10-11 | 三井化学株式会社 | エチレン系共重合体組成物およびその用途 |
| JP2023043417A (ja) * | 2021-09-16 | 2023-03-29 | バンドー化学株式会社 | ゴム-繊維複合体及びその製造方法、並びにそれを含むコンベヤベルト |
| JP2025075456A (ja) * | 2023-10-31 | 2025-05-15 | 三井化学株式会社 | 伝動ベルト用組成物およびその用途 |
| JP2025075455A (ja) * | 2023-10-31 | 2025-05-15 | 三井化学株式会社 | 伝動ベルト用組成物およびその用途 |
-
2025
- 2025-06-06 JP JP2025533435A patent/JPWO2026028601A1/ja active Pending
- 2025-06-06 WO PCT/JP2025/020496 patent/WO2026028601A1/ja active Pending
Patent Citations (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2006138355A (ja) * | 2004-11-10 | 2006-06-01 | Bando Chem Ind Ltd | 伝動ベルト |
| JP2009137272A (ja) * | 2007-11-16 | 2009-06-25 | Toyoda Gosei Co Ltd | ウォーターホース及びホース用混合物 |
| WO2015122415A1 (ja) * | 2014-02-13 | 2015-08-20 | 三井化学株式会社 | エチレン・α-オレフィン・非共役ポリエン共重合体およびその用途、並びにその製造方法 |
| WO2021006018A1 (ja) * | 2019-07-08 | 2021-01-14 | Nok株式会社 | トーショナルダンパ用ゴム組成物 |
| JP2021080440A (ja) * | 2019-11-20 | 2021-05-27 | 三ツ星ベルト株式会社 | 成形用部材およびその用途 |
| JP2021161345A (ja) * | 2020-04-02 | 2021-10-11 | 三井化学株式会社 | エチレン系共重合体組成物およびその用途 |
| JP2023043417A (ja) * | 2021-09-16 | 2023-03-29 | バンドー化学株式会社 | ゴム-繊維複合体及びその製造方法、並びにそれを含むコンベヤベルト |
| JP2025075456A (ja) * | 2023-10-31 | 2025-05-15 | 三井化学株式会社 | 伝動ベルト用組成物およびその用途 |
| JP2025075455A (ja) * | 2023-10-31 | 2025-05-15 | 三井化学株式会社 | 伝動ベルト用組成物およびその用途 |
Also Published As
| Publication number | Publication date |
|---|---|
| JPWO2026028601A1 (cg-RX-API-DMAC7.html) | 2026-02-05 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| CN101357786B (zh) | 水性处理剂 | |
| JP6549902B2 (ja) | ダイシングダイボンドフィルム、半導体装置の製造方法および半導体装置 | |
| JPWO2007110974A1 (ja) | 伝動ベルト | |
| JP6733436B2 (ja) | 接着剤、加硫ゴム接着方法、コンベヤベルト | |
| BR112013007035B1 (pt) | Processo para fabricar um artigo de multicamadas | |
| JP7724666B2 (ja) | ゴム-繊維複合体及びその製造方法、並びにそれを含むコンベヤベルト | |
| JP2026042950A (ja) | 架橋ゴム組成物及びそれを用いた伝動ベルト | |
| JP4651767B2 (ja) | 固形タイプの粘着剤組成物とその粘着シ―ト類 | |
| WO2026028603A1 (ja) | 架橋ゴム組成物及びそれを用いた伝動ベルト | |
| CN116348542A (zh) | 交联橡胶组合物及使用该交联橡胶组合物的摩擦传动带 | |
| KR101820319B1 (ko) | 접착 방법 및 컨베이어 벨트 | |
| JP4698342B2 (ja) | ゴム組成物ならびにゴム組成物が用いられた搬送ベルト | |
| JP7457593B2 (ja) | ゴム繊維複合体 | |
| JPS61111332A (ja) | ゴム組成物の接着方法 | |
| JP6424599B2 (ja) | 接着方法およびコンベヤベルト | |
| JPS60215085A (ja) | 溶液状加硫型ゴム接着剤 | |
| JP5851852B2 (ja) | 加硫ゴムと樹脂の積層体及び積層体の製造方法 | |
| JP4899495B2 (ja) | ガラス繊維被覆用塗布液およびそれを用いたゴム補強用ガラス繊維 | |
| CN108699413B (zh) | 粘接剂用橡胶组合物、橡胶的粘接方法以及传送带 | |
| JP4752614B2 (ja) | 繊維被覆用塗布液およびそれを用いたゴム補強用繊維 | |
| JP6435710B2 (ja) | 接着方法およびコンベヤベルト | |
| KR100394547B1 (ko) | 이피디엠(epdm)고무의 물성을 향상시키는 방법 | |
| JPH01193383A (ja) | 接着剤 | |
| JP5037801B2 (ja) | ゴム組成物が用いられた搬送ベルト | |
| JP5820229B2 (ja) | 加硫ゴムと樹脂部材の接着方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| ENP | Entry into the national phase |
Ref document number: 2025533435 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2025533435 Country of ref document: JP |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 25847754 Country of ref document: EP Kind code of ref document: A1 |