WO2025256322A1 - 电子设备的壳体及其制作方法、电子设备 - Google Patents
电子设备的壳体及其制作方法、电子设备Info
- Publication number
- WO2025256322A1 WO2025256322A1 PCT/CN2025/094696 CN2025094696W WO2025256322A1 WO 2025256322 A1 WO2025256322 A1 WO 2025256322A1 CN 2025094696 W CN2025094696 W CN 2025094696W WO 2025256322 A1 WO2025256322 A1 WO 2025256322A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- substrate
- cellulose acetate
- housing
- electronic device
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本申请提供一种电子设备的壳体及其制作方法、电子设备,涉及电子产品技术领域。壳体在基体的内表面依次设置有醋酸纤维膜和防护层,醋酸纤维膜可以赋予壳体独特的纹理和光泽。通过将基体和防护层设置为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,基体和防护层均采用塑料制作而成,可以降低壳体的制作成本,进而节约电子设备整机的生产成本。并且,通过将醋酸纤维膜夹设在基体和防护层之间,可以从两侧对醋酸纤维膜进行保护,且可以减少醋酸纤维膜两侧的空隙,增强壳体的密实度。进而,提升壳体的防水性能,提升壳体及电子设备整机的可靠性。
Description
本申请要求于2024年06月14日提交中国专利局、申请号为202410775896.4、申请名称为“电子设备的壳体及其制作方法、电子设备”的中国专利申请的优先权,其全部内容通过引用结合在本申请中。
本申请涉及电子产品技术领域,特别涉及一种电子设备的壳体及其制作方法、电子设备。
电子设备的壳体主要采用金属、玻璃、塑料或陶瓷等材质,由于金属壳体的信号透过能力有限,随着5G时代的来临,越来越多的生产厂商选择信号透过能力强的玻璃或塑料制作壳体。
为了呈现较好的外观效果,一些电子设备的壳体采用玻璃作为基体,采用光学透明胶粘剂(Optically Clear Adhesive,简称OCA)在玻璃的内表面贴附醋酸纤维膜,以通过醋酸纤维膜在壳体中注入天然矿物粉,赋予壳体独特的纹理和光泽。醋酸纤维膜之上设置油墨层作为壳体的盖底层。盖底层和醋酸纤维膜之间还可以设置镀膜层、UV纹理层等结构层,以增强壳体的色彩效果。
然而,现有电子设备的壳体的制作成本高,有些还存在防水性能差、影响醋酸纤维膜的纹理效果等问题。
本申请提供一种电子设备的壳体及其制作方法、电子设备,电子设备的壳体具有纹理和光泽,且制作成本低、防水性能好,电子设备的外观效果好、成本低且可靠性高。
本申请的第一方面提供一种电子设备的壳体,包括:基体,包括相对设置的外表面和内表面;基体为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板;醋酸纤维膜,设置在基体的内表面所在的一侧;防护层,设置在醋酸纤维膜背离基体的一侧;防护层为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板。
本申请的电子设备的壳体,以基体作为主要支撑结构,基体的外表面朝向外界、基体的内表面朝向电子设备内部,基体的内表面依次设置有醋酸纤维膜和防护层。通过在壳体中加入醋酸纤维膜,醋酸纤维膜可以赋予壳体独特的纹理和光泽。通过将基体和防护层设置为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,基体和防护层均采用塑料制作而成,可以降低壳体的制作成本,进而节约电子设备整机的生产成本。并且,通过将醋酸纤维膜夹设在基体和防护层之间,可以从两侧对醋酸纤维膜进行保护,且有利于减少醋酸纤维膜两侧的空隙,增强醋酸纤维膜两侧的密实度。进而,提升壳体的防水性能,防止因醋酸纤维膜吸水而影响壳体的外观效果,提升壳体及电子设备整机的可靠性。
在一种可能的实施方式中,基体和醋酸纤维膜之间设置有第一胶层,防护层和醋酸纤维膜之间设置有第二胶层。
通过第一胶层和第二胶层分别将基体和防护层粘接在醋酸纤维膜的两侧,保证基体、醋酸纤维膜及防护层三者的连接强度。并且,通过第一胶层和第二胶层将醋酸纤维膜夹住,外加基体和防护层均为高密度的结构件,可以减少醋酸纤维膜两侧的空隙,保证醋酸纤维膜两侧的密实度,提升壳体的防水性能,避免醋酸纤维膜进水,保证壳体的外观效果。
在一种可能的实施方式中,第一胶层和第二胶层中的至少一者为UV胶层。
通过将第一胶层和第二胶层中的至少一者设置为UV胶层,UV胶的固化方式简单、固化速度快且成本低,可以提升壳体的制作效率,降低壳体的制作成本。
在一种可能的实施方式中,基体的厚度范围为0.30mm-0.45mm,防护层的厚度范围为0.05mm-0.15mm。
通过将基体的厚度设置在0.03mm-0.45mm之间,基体具有足够的厚度,满足基体的结构强度需求。并且,基体的厚度不至于过大,可以减小壳体的厚度。通过将防护层的厚度设置在0.05mm-0.15mm之间,防护层的厚度不至于过小,防护层具有足够的结构强度和稳定性,能够支撑醋酸纤维膜,防止外界水汽进入醋酸纤维膜。并且,防护层的厚度小于基体的厚度,可以减薄壳体的整体厚度。
在一种可能的实施方式中,醋酸纤维膜的厚度范围为0.05mm-0.15mm。
通过将醋酸纤维膜的厚度设置在0.05mm-0.15mm之间,醋酸纤维膜具有一定的厚度,可以保证醋酸纤维膜的结构强度和稳定性,保证醋酸纤维膜的纹理效果和光泽度,避免其他结构层对壳体的外观效果造成影响。并且,醋酸纤维膜的厚度较小,可以避免醋酸纤维膜过厚而影响壳体的结构强度。
在一种可能的实施方式中,电子设备的壳体还包括:盖底层,设置在防护层背离醋酸纤维膜的一侧。
通过在防护层背离醋酸纤维膜的一侧设置盖底层,盖底层可以位于壳体朝向电子设备内的一侧表面。盖底层作为壳体的内表层,通常为印刷或喷涂的油墨层,可以对壳体进行保护,防止盖底层之下的结构层被磨损或刮花。
在一种可能的实施方式中,电子设备的壳体还包括:至少一层镀膜层,设置在盖底层和防护层之间。
通过在盖底层和防护层之间设置至少一层镀膜层,可以增强壳体的硬度、抗氧化性、耐久性、散热性的性能。从而,提升壳体的稳定性和可靠性,延长壳体的使用寿命。
在一种可能的实施方式中,至少一层镀膜层包括:氧化硅层,附着于盖底层;氧化锆层,设置于氧化硅层和防护层之间。
在一种可能的实施方式中,氧化硅层和氧化锆层之间设置有油墨层。
在一种可能的实施方式中,电子设备的壳体还包括:UV纹理层,设置在防护层和镀膜层之间。
通过在防护层和镀膜层之间设置UV纹理层,UV纹理层可以通过UV转印方式形成在防护层上。如此,可以增强镀膜层与防护层之间附着力,提升壳体的整体性和可靠性。在有些情况下,UV纹理层还可以与醋酸纤维膜的纹理效果叠加,可以提升壳体的外观效果。
在一种可能的实施方式中,电子设备的壳体还包括:强化层,设置在基体的外表面。
通过在基体的外表面设置强化层,强化层作为壳体的外表层,主要用于对壳体的外表面进行加硬处理,以增强壳体的硬度和耐磨性。从而,提升壳体的稳定性和可靠性,延长壳体的使用寿命。
本申请的第二方面提供一种电子设备的壳体的制作方法,包括:提供基体和醋酸纤维膜,并将基体的内表面和醋酸纤维膜贴合连接;提供防护层,并将防护层贴合在醋酸纤维膜背离基体的一侧表面;其中,基体和防护层分别为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板。
本申请的壳体的制作方法,通过提供基体、醋酸纤维膜及防护层,将基体的内表面与醋酸纤维膜贴合连接,将防护层贴合在醋酸纤维膜背离基体的一侧表面。通过在壳体中加入醋酸纤维膜,醋酸纤维膜可以赋予壳体独特的纹理和光泽。通过将基体和防护层设置为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,基体和防护层均采用塑料制作而成,可以降低壳体的制作成本,进而节约电子设备整机的生产成本。并且,通过将醋酸纤维膜夹设在基体和防护层之间,可以从两侧对醋酸纤维膜进行保护,且有利于减少醋酸纤维膜两侧的空隙,增强醋酸纤维膜两侧的密实度。进而,提升壳体的防水性能,防止因醋酸纤维膜吸水而影响壳体的外观效果,提升壳体及电子设备整机的可靠性。
在一种可能的实施方式中,将基体和醋酸纤维膜贴合连接,包括:在基体和醋酸纤维膜中的一者的表面上形成第一胶层;将基体和醋酸纤维膜通过第一胶层贴合连接;和/或,将防护层贴合在醋酸纤维膜背离基体的一侧表面,包括:在醋酸纤维膜背离基体的一侧表面上形成第二胶层;将防护层通过第二胶层贴合在醋酸纤维膜背离基体的一侧表面。
在一种可能的实施方式中,当基体为聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,且第一胶层为UV胶层时,将基体和醋酸纤维膜通过第一胶层贴合连接,包括:将紫外灯设置在醋酸纤维膜所在的一侧,使紫外灯发出的紫外光穿过醋酸纤维膜到达第一胶层,以将第一胶层固化。
当第一胶层为UV胶层时,需要通过紫外光对第一胶层进行固化。当基体为聚甲基丙烯酸甲酯层或复合板,相较于基体,醋酸纤维膜对紫外光的透过率更高。通过将紫外灯设置在醋酸纤维膜所在的一侧,紫外灯发出的紫外光穿过醋酸纤维膜到达第一胶层。以确保第一胶层对紫外光的吸收率,保证第一胶层固化完全。
在一种可能的实施方式中,当防护层为聚碳酸酯层,且第二胶层为UV胶层时,将防护层贴合在醋酸纤维膜背离基体的一侧表面,包括:将紫外灯设置在防护层所在的一侧,使紫外灯发出的紫外光穿过防护层到达第二胶层,以将第二胶层固化。
当第二胶层为UV胶层时,需要通过紫外光对第二胶层进行固化。当防护层为聚碳酸酯层时,防护层对紫外光的透过率很高。通过将紫外灯设置在防护层所在的一侧,紫外光穿过防护层到达第二胶层。以确保第二胶层对紫外光的吸收率,保证第二胶层完全固化。并且,紫外光穿透的结构层较少,第二胶层对紫外光的吸收速率快,第二胶层的固化速率高。
在一种可能的实施方式中,当基体为聚碳酸酯层,防护层为聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,且第二胶层为UV胶层时,将防护层贴合在醋酸纤维膜背离基体的一侧表面,包括:将紫外灯设置在基体所在的一侧,使紫外灯发出的紫外光依次穿过基体、第一胶层及醋酸纤维膜到达第二胶层,以将第二胶层固化。
当第二胶层为UV胶层时,需要通过紫外光对第二胶层进行固化。当基体为聚碳酸酯层、防护层为聚甲基丙烯酸甲酯层或复合板时,相较于防护层,基体对紫外光的透过率更高。通过将紫外灯设置在基体所在的一侧,紫外光依次穿过基体、第一胶层及醋酸纤维膜到达第二胶层。以确保第二胶层对紫外光的吸收率,保证第二胶层完全固化。
在一种可能的实施方式中,壳体的制作方法还包括:在防护层背离醋酸纤维膜的一侧形成盖底层。
在一种可能的实施方式中,壳体的制作方法还包括:在盖底层和防护层之间形成至少一层镀膜层。
在一种可能的实施方式中,壳体的制作方法还包括:在防护层和镀膜层之间形成UV纹理层。
在一种可能的实施方式中,壳体的制作方法还包括:在基体的外表面形成强化层。
本申请的第三方面提供一种电子设备,包括显示屏和如前所述的壳体,显示屏安装于壳体。
本申请的电子设备,包括壳体和安装于壳体的显示屏,壳体以基体作为主要支撑结构,基体的外表面朝向外界、基体的内表面朝向电子设备内部,基体的内表面依次设置有醋酸纤维膜和防护层。通过在壳体中加入醋酸纤维膜,醋酸纤维膜可以赋予壳体独特的纹理和光泽。通过将基体和防护层设置为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,基体和防护层均采用塑料制作而成,可以降低壳体的制作成本,进而节约电子设备整机的生产成本。并且,通过将醋酸纤维膜夹设在基体和防护层之间,可以从两侧对醋酸纤维膜进行保护,且有利于减少醋酸纤维膜两侧的空隙,增强醋酸纤维膜两侧的密实度。进而,提升壳体的防水性能,防止因醋酸纤维膜吸水而影响壳体的外观效果,提升壳体及电子设备整机的可靠性。
图1为本申请实施例提供的一种电子设备的结构示意图;
图2为图1所示的电子设备的分解结构图;
图3为本申请实施例提供的另一种电子设备的结构示意图;
图4为图3中的电子设备处于折叠状态时的结构示意图;
图5为图3中的电子设备处于展开状态时的结构示意图;
图6为图3中的电子设备的分解结构图;
图7为本申请实施例提供的第一种壳体的结构示意图;
图8为本申请实施例提供的第二种壳体的结构示意图;
图9为本申请实施例提供的第三种壳体的结构示意图;
图10为本申请实施例提供的第四种壳体的结构示意图;
图11为本申请实施例提供的第五种壳体的结构示意图;
图12为本申请实施例提供的壳体的制作方法的步骤流程图。
附图标记说明:
10-电子设备;
100-显示屏;200-壳体;300-电路板;400-电池;500-摄像头;
110-折叠屏;120-直板屏;210-第一壳体;220-第二壳体;230-转轴机构;
111-第一非弯折部;112-可弯折部;113-第二非弯折部;201-中框;202-后盖;
2001-基体;2002-醋酸纤维膜;2003-防护层;2004-第一胶层;2005-第二胶层;2006-盖底层;2007-强
化层;2008-镀膜层;2009-油墨层;2010-UV纹理层;
20081-氧化硅层;20082-氧化锆层;
a-聚碳酸酯层;b-聚甲基丙烯酸甲酯层。
10-电子设备;
100-显示屏;200-壳体;300-电路板;400-电池;500-摄像头;
110-折叠屏;120-直板屏;210-第一壳体;220-第二壳体;230-转轴机构;
111-第一非弯折部;112-可弯折部;113-第二非弯折部;201-中框;202-后盖;
2001-基体;2002-醋酸纤维膜;2003-防护层;2004-第一胶层;2005-第二胶层;2006-盖底层;2007-强
化层;2008-镀膜层;2009-油墨层;2010-UV纹理层;
20081-氧化硅层;20082-氧化锆层;
a-聚碳酸酯层;b-聚甲基丙烯酸甲酯层。
本申请的实施方式部分使用的术语仅用于对本申请的具体实施例进行解释,而非旨在限定本申请。
本申请实施例提供一种电子设备,电子设备可以为消费类电子产品。示例性的,电子设备包括但不限于为手机、平板电脑(portable android device,PAD)、笔记本电脑、膝上型电脑(laptop computer)、上网本、超级移动个人计算机(ultra-mobile personal computer,UMPC)、对讲机、POS(Point of sales)机、个人数字助理(personal digital assistant,PDA)、多媒体播放器、电子书阅读器、车载设备、可穿戴设备、虚拟现实(virtual reality,VR)设备、增强现实(augmented reality,AR)设备等。其中,可穿戴设备包括但不限于智能手环、智能手表、智能头戴显示器、智能眼镜等。
图1为本申请实施例提供的一种电子设备的结构示意图。参照图1所示,以电子设备10为直板式电子设备为例,例如,电子设备10为直板手机,电子设备10可以包括显示屏100和壳体200。显示屏100的一侧表面用于显示图像信息,通常将显示屏100的该侧表面定义为其正面,与其正面相背的另一侧表面为其背面。壳体200围设在显示屏100的周侧和背面,用于对显示屏100进行支撑固定,并提供保护。显示屏100的正面暴露在壳体200之外,以供用户观看显示屏100显示的内容或对电子设备10进行输入操作。
图2为图1所示的电子设备的分解结构图。参照图2所示,当电子设备10为直板式电子设备时,该电子设备10的壳体200可以包括中框201和后盖202,中框201连接在显示屏100和后盖202之间,显示屏100支撑在中框201的一侧表面,后盖202连接在中框201的另一侧表面。
其中,显示屏100通常是整体贴装在中框201上,以保证显示屏100的强度和稳定性,满足显示屏100的使用要求。后盖202通常采用搭接的方式与中框201连接,中框201和后盖202共同围成收容腔,收容腔内用于安装电路板300、电池400、摄像头500、扬声器(图中未示出)等器件。
图3为本申请实施例提供的另一种电子设备的结构示意图。图4为图3中的电子设备处于折叠状态时的结构示意图。图5为图3中的电子设备处于展开状态时的结构示意图。
参照图3至图5所示,以电子设备10为折叠式电子设备为例,例如,电子设备10为折叠手机,电子设备10可以包括能够相对转动的至少两个部分,在不同的使用场景下,电子设备10可以具有不同的使用状态。本实施例以折叠式电子设备为可发生一次折叠的电子设备10为例,电子设备10包括能够相互转动的两个部分,通过两个部分的相对转动,改变电子设备10的使用状态。
其中,电子设备10的两个部分可以沿图3中所示的箭头方向相对转动,当两个部分转动至相互层叠时,电子设备10处于图4中示出的折叠状态。此时,电子设备10的体积较小,便于携带。电子设备10的两个部分也可以沿与图3中的箭头方向相反的方向相对转动,当两个部分转动至共面时,电子设备10处于图5中示出的展开状态,电子设备10的展开角度α例如为180°。此时,电子设备10可以实现大屏显示。
需要说明的是,本实施例举例说明的角度均允许存在少许偏差。例如,电子设备10的展开角度α为180°是指,展开角度α可以为180°,也可以为大约180°,比如170°、175°、185°或190°等。后文中举例说明的角度可做相同理解。
另外,除了可发生一次折叠的电子设备10外,电子设备10也可以为可发生两次以上折叠的电子设备10。此时,电子设备10可以包括依次转动连接的多个部分,相邻两个部分可相对靠近以折叠至折叠状态,相邻两个部分也可以相对远离以展开至展开状态。
图6为图3中的电子设备的分解结构图。参照图6所示,对于折叠式电子设备,电子设备10同样也可以包括显示屏100和壳体200。显示屏100的正面用于显示图像信息,壳体200围设在显示屏100的周侧和背面,用于对显示屏100进行支撑固定,并提供保护,此处不再赘述。
电子设备10的显示屏100可以包括折叠屏110,折叠屏110可以包括沿第一方向依次设置的第一非弯折部111、可弯折部112和第二非弯折部113。或者说,在第一方向上,可弯折部112位于第一非弯折部111和第二非弯折部113之间。其中,电子设备10的折叠方式可以为图3至图5中所示的横向折叠,此时,第一方向可以为图6中所示的X方向。当然,电子设备10的折叠方式也可以为竖向折叠,本实施例对此不作限制。
示例性的,折叠屏110可以采用柔性材料制作,以使可弯折部112可弯折。折叠屏110可以为有机发光二极管(organic light-emitting diode,OLED)显示屏100。
壳体200用于支撑和固定折叠屏110,并带动折叠屏110在折叠状态与展开状态之间切换。参照图6所示,壳体200包括第一壳体210、第二壳体220和转轴机构230,转轴机构230连接在第一壳体210和第二壳体220之间,第一壳体210和第二壳体220通过转轴机构230实现可转动连接,从而,实现第一壳体210和第二壳体220之间的相对转动。
第一壳体210支撑并固定折叠屏110的第一非弯折部111,第二壳体220支撑并固定折叠屏110的第二非弯折部113,转轴机构230支撑折叠屏110的可弯折部112。换言之,折叠屏110的第一非弯折部111固定连接于第一壳体210,折叠屏110的第二非弯折部113固定连接于第二壳体220,折叠屏110的可弯折部112对应转轴机构230设置。
电子设备10在使用过程中,折叠屏110的第一非弯折部111和第二非弯折部113始终保持平面状态,而折叠屏110的可弯折部112可以发生弯折。转轴机构230带动第一壳体210和第二壳体220相对转动时,折叠屏110的第一非弯折部111和第二非弯折部113随之改变方位,折叠屏110的可弯折部112随第一非弯折部111和第二非弯折部113的方位改变而折弯或展平。
其中,第一壳体210和第二壳体220可以向相互靠近的方向转动,至两者相对层叠。此时,壳体200处于折叠状态,折叠屏110随壳体200的折叠而处于折叠状态(如图4所示)。第一壳体210和第二壳体220也可以向相互远离的方向转动,至两者共面。此时,壳体200处于展开状态,折叠屏110随壳体200的展开而处于展开状态(如图5所示)。
应说明,本实施例以电子设备10为内折式电子设备为例,当电子设备10处于折叠状态时,折叠屏110的第一非弯折部111和第二非弯折部113相对贴合,壳体200围设在折叠屏110外,折叠屏110位于第一壳体210和第二壳体220之间。如此,内折式电子设备处于折叠状态时,壳体200可以为折叠屏110=提供保护,以防止折叠屏110被硬物刮伤。
若内折式电子设备需要在折叠状态下实现显示功能,可以在壳体200的背面增设一块直板屏120,电子设备10在折叠状态下,依靠该直板屏120实现显示功能(参见图3或图4)。换言之,内折式电子设备的显示屏100可以包括折叠屏110和直板屏120。折叠屏110可以贴装在壳体200的正面,随着壳体200的运动,折叠屏110可以在展开状态和折叠状态之间切换。电子设备10处于折叠状态时,折叠屏110对外不可见。直板屏120可以贴装在壳体200的背面,直板屏120在电子设备10处于折叠状态时进行显示。
在其他示例中,电子设备10也可以为外折式电子设备,当电子设备10处于折叠状态时,折叠屏110的第一非弯折部111和第二非弯折部113相背,壳体200位于第一非弯折部111和第二非弯折部113之间。换言之,外折式电子设备处于折叠状态时,折叠屏110围设在第一壳体210和第二壳体220外,折叠屏110对用户可见,可以利用折叠屏110实现显示功能。因而,无需为了实现电子设备10在折叠状态下的显示功能,而额外在壳体200的背面增加直板屏120。
另外,在有些实施方式中,电子设备10尤其是内折式电子设备,可以悬停在展开状态与折叠状态之间的某一角度β(参见图3所示)。示例性的,电子设备10的悬停角度β可以为120°、130°、140°或150°等。其中,可以依靠壳体200提供的阻尼力,使得壳体200悬停在折叠状态与展开状态之间的半展开状态,折叠屏110随壳体200停留在半展开状态。
此时,折叠屏110的可弯折部112也处于折弯状态,并且,可弯折部112的折弯程度小于处于折叠状态时的折弯程度。折叠屏110的第一非弯折部111和第二非弯折部113之间相对倾斜,第一非弯折部111和第二非弯折部113之间的夹角例如为120°、130°、140°或150°等。
继续参照图6,折叠式电子设备的壳体200中,第一壳体210和第二壳体220均可以包括中框201,折叠屏110的第一非弯折部111和第二非弯折部113可以支撑在对应中框201的正面。其中,对于外折式电子设备或未额外设置直板屏120的内折式电子设备,电子设备10的第一壳体210和第二壳体220均还可以包括后盖202,后盖202连接在中框201背离折叠屏110的一侧表面。对于额外设置了直板屏120的内折式电子设备,第一壳体210和第二壳体220中的一者可以不包括后盖202,而是作为替代在中框201的背面安装直板屏120。
第一壳体210和第二壳体220中,中框201和后盖202(或直板屏120)共同围成收容腔,收容腔内用于安装电路板300、电池400、摄像头500、扬声器(图中未示出)等器件。
正如背景技术中所述,相关技术中,一些电子设备10的壳体200采用玻璃作为基体2001,并采用OCA胶层在玻璃的内表面附着醋酸纤维膜2002,以通过醋酸纤维膜2002赋予壳体200独特的纹理和光泽。然而,由于玻璃、OCA胶层的成本较高,现有的壳体200的制作成本通常较高,不利于电子设备10整机的成本控制。并且,在壳体200组装至电子设备10整机之前,以及壳体200在电子设备10整机中服役的过程中,还存在醋酸纤维膜2002易吸水而影响壳体200的外观效果、可靠性的问题。
有鉴于此,本申请实施例对电子设备10的壳体200进行改进,壳体200以基体作为主要支撑结构,基体的外表面朝向外界、基体的内表面朝向电子设备10内部,基体的内表面依次设置有醋酸纤维膜和防护层。通过在壳体200中加入醋酸纤维膜,醋酸纤维膜可以赋予壳体200独特的纹理和光泽。通过将基体和防护层设置为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,基体和防护层均采用塑料制作而成,可以降低壳体200的制作成本,进而节约电子设备10整机的生产成本。并且,通过将醋酸纤维膜夹设在基体和防护层之间,可以从两侧对醋酸纤维膜进行保护,且有利于减少醋酸纤维膜两侧的空隙,增强醋酸纤维膜两侧的密实度。进而,提升壳体200的防水性能,防止因醋酸纤维膜吸水而影响壳体200的外观效果,提升壳体200及电子设备10整机的可靠性。
以下对本申请实施例的电子设备10的壳体200进行详细说明。
以电子设备10为前述直板式电子设备为例,具体可以是对壳体200中的后盖202进行改进。以电子设备10为前述折叠式电子设备为例,具体可以是对第一壳体210和第二壳体220中的后盖202进行改进。当电子设备10为平板电脑、笔记本电脑或可穿戴设备等其他电子产品时,可以是对电子设备10中作为外观件的壳体200进行改进。
图7为本申请实施例提供的第一种壳体的结构示意图。图8为本申请实施例提供的第二种壳体的结构示意图。图9为本申请实施例提供的第三种壳体的结构示意图。图10为本申请实施例提供的第四种壳体的结构示意图。
参照图7至图10任一所示,本实施例中,壳体200可以包括依次层叠设置的基体2001、醋酸纤维膜2002和防护层2003。基体2001厚度方向的两侧表面分别为外表面和内表面,基体2001的外表面朝向外界,基体2001的内表面朝向电子设备10内部。以前述的电子设备10中的后盖202为例,基体2001的外表面可以背向中框201,而基体2001的内表面则可以朝向中框201。醋酸纤维膜2002和防护层2003依次设置在基体2001的内表面所在的一侧。
基体2001可以为壳体200中的支撑主体,其作为壳体200的主要承力结构,用于使壳体200具有足够的结构强度,以保证壳体200的稳定性和可靠性,保障壳体200的使用寿命。基体2001可以具有一定的厚度,且基体2001具有良好的硬度和机械强度,以提供壳体200所需的结构强度。
基体2001可以为透明结构,基体2001的透光率可以达到90%以上,壳体200的外观效果主要由位于基体2001内侧的醋酸纤维膜2002呈现。醋酸纤维膜2002是醋酸纤维制作而成的薄膜,而醋酸纤维是以醋酸作为溶剂、醋酐作为乙酰化剂,在催化剂作用下进行酯化,而得到的热塑性树脂。由醋酸纤维制作而成的醋酸纤维膜2002,具有层次感佳、光泽度好、不易变形变色、经久耐用的优点。通过在基体2001的内侧设置醋酸纤维膜2002,可以赋予壳体200特殊的纹理和光泽,可以提升壳体200的外观效果。
示例性的,醋酸纤维膜2002可以是将粉末状的醋酸纤维原料,经过配比、搅拌、揉捏、混料、压板成型、裁切等一系列工序而形成的膜片。可以将不同颜色的色粉(有颜色的粉末物质)与醋酸纤维原料混合,形成至少两种不同颜色的醋酸纤维原料。然后,将不同颜色的醋酸纤维原料制作成为大颗粒件或小尺寸薄片件,再将这些大颗粒件或小尺寸薄片件混合或摆放定型后,压板成型为尺寸较大、厚度较大的醋酸纤维板。之后,再将醋酸纤维板经过拉伸和裁切等工序,形成具有合适尺寸和厚度的醋酸纤维膜2002。
制作醋酸纤维膜2002的原料中还可以加入天然矿物粉,可以将天然矿物粉混入醋酸纤维原料中形成粉末状原料。天然矿物粉的加入,可以使醋酸纤维膜2002呈现出特殊的自然纹理和光泽度,以提升壳体200的外观效果。例如,可以将天然贝母材料混入醋酸纤维原料中,使壳体200呈现出非常接近珍珠的光泽度。
可以理解的是,通过在醋酸纤维原料中加入天然矿物粉,使得醋酸纤维膜2002呈现出非常接近自然的纹理和光泽度。同时,利用醋酸纤维原料自身塑性好、形变能力强的特点,使得醋酸纤维膜2002易于拉伸变形,可以形成无限变化、独一无二的纹理效果。
其中,通过对压板成型后的醋酸纤维板进行拉伸,例如,对醋酸纤维板进行横向拉伸和纵向拉伸,不仅可以将醋酸纤维板的厚度减薄,使之形成为厚度较薄的醋酸纤维膜2002。并且,醋酸纤维板上的纹理的走向、轮廓及光泽都会随之改变,最终形成的每个醋酸纤维膜2002呈现的纹理和光泽都是独一无二的。从而,配置有该壳体200的每个电子设备10,都可以呈现独一无二的外观效果。
以醋酸纤维膜2002具有两种不同颜色的粉末状原料为例,该两种不同颜色的粉末状原料的颜色可以接近,醋酸纤维膜2002形成的纹理可以深浅不一或明暗相间。从而,电子设备10的壳体200具有色系接近且明暗相间的纹理效果。或者,该两种不同颜色的醋酸纤维原料的颜色可以具有较大差异,醋酸纤维膜2002形成的纹理可以双色相间、变化独特。从而,电子设备10的壳体200具有双色相间、视觉独特的纹理效果。
由于醋酸纤维膜2002以醋酸纤维作为基体2001材料,相较于密度较大、硬度较高的板材而言,醋酸纤维膜2002易吸水。而醋酸纤维膜2002若吸水过多,会影响醋酸纤维膜2002的纹理和光泽,进而影响壳体200的外观效果。若醋酸纤维膜2002吸水过多,还可能会影响醋酸纤维膜2002与其两侧的结构层的连接强度,进而影响壳体200的稳定性和可靠性,影响壳体200的使用寿命。
对此,本实施例在醋酸纤维膜2002背离基体2001的一侧还设置了防护层2003,防护层2003也可以具有一定厚度,且防护层2003具有良好的硬度和机械强度。基体2001和防护层2003将醋酸纤维膜2002夹设在两者之间,形成三明治结构。基体2001和防护层2003分别紧密贴合在醋酸纤维膜2002的两侧,对于具有足够硬度和机械强度的基体2001和防护层2003而言,基体2001和防护层2003的密度均较大,可以减少醋酸纤维膜2002两侧存在的空隙,保证醋酸纤维膜2002两侧的密实度,从而对醋酸纤维膜2002的两侧进行防护。
从而,通过基体2001和防护层2003将醋酸纤维膜2002夹设其间这样的三明治结构,可以提升壳体200的防水性能。防止外界水汽进入醋酸纤维膜2002,避免醋酸纤维膜2002吸水而影响纹理和光泽,保证壳体200的外观效果。并且,保证醋酸纤维膜2002与其两侧的基体2001及防护层2003的连接强度,提升壳体200的稳定性和可靠性,延长壳体200的使用寿命。
示例性的,在电子设备10的使用过程中,由于醋酸纤维膜2002的两侧分别与基体2001及防护层2003紧密贴合,醋酸纤维膜2002两侧的空隙很少,醋酸纤维膜2002两侧的密实度高。可以防止外界水汽从壳体200的外表面(基体2001所在的一侧)进入醋酸纤维膜2002。并且,由于醋酸纤维膜2002两侧的空隙很少,醋酸纤维膜2002与其两侧的基体2001、防护层2003构成的三明治结构的整体密度大,也可以防止外界水汽从壳体200的周侧进入醋酸纤维膜2002,防止壳体200的侧壁进水,避免壳体200和中框201的装配方式导致的进水问题。
在壳体200组装至电子设备10之前,通过基体2001和防护层2003将醋酸纤维膜2002夹设其间这样的三明治结构,也可以防止外界水汽从壳体200的两侧表面进入醋酸纤维膜2002。保证醋酸纤维膜2002的纹理和光泽效果,保证壳体200的外观强度。并且,防护层2003可以增强壳体200的结构强度,醋酸纤维膜2002与其两侧的基体2001及防护层2003的连接强度高,可以提升壳体200的稳定性和可靠性,防止壳体200受到损伤。
其中,基体2001可以采用聚碳酸酯(Polycarbonate,简称PC)制作而成,基体2001为聚碳酸酯层a。聚碳酸酯的透明度高,满足基体2001的透光度需求。同时,聚碳酸酯还具有冲击强度高、韧性好、耐疲劳性佳、尺寸稳定性好、使用温度范围广的其他优点,可以提升壳体200的可靠性和使用寿命。
或者,基体2001也可以采用聚甲基丙烯酸甲酯(poly(methyl methacrylate),简称PMMA))制作而成,基体2001为聚甲基丙烯酸甲酯层b。聚甲基丙烯酸甲酯的透明度高,满足基体2001的透光度需求。同时,聚甲基丙烯酸甲酯还具有高强度、高硬度、耐磨性好、尺寸稳定性好等其他优点,可以提升壳体200的可靠性和使用寿命。
又或者,基体2001可以由聚碳酸酯和聚甲基丙烯酸甲酯复合而成,基体2001为由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板。这样,在保证基体2001的高透光率的基础上,作为基体2001的复合板,既具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性,可以进一步提升壳体200的可靠性和使用寿命。
当基体2001为由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板时,可以将聚碳酸酯层a和聚甲基丙烯酸甲酯层b经过共挤,挤压成型为复合板而作为基体2001。这样,基体2001的层与层之间无需使用粘合剂,基体2001的整体性好、结构强度高,有利于提升壳体200的稳定性和可靠性。并且,由于不使用粘合剂,不存在溶剂残留问题,基体2001无异味。
以基体2001包括一层聚碳酸酯层a和一层聚甲基丙烯酸甲酯层b为例,可以将聚甲基丙烯酸甲酯层b设置在基体2001的外表面所在的一侧,以保证壳体200的硬度和耐磨性。将聚碳酸酯层a设置在基体2001的内表面所在的一侧,以保证基体2001的冲击韧性,提升壳体200整体的冲击韧性。
与基体2001类似的,防护层2003可以采用聚碳酸酯制作而成,防护层2003为聚碳酸酯层a,防护层2003的冲击强度高、韧性好。或者,防护层2003可以采用聚甲基丙烯酸甲酯制作而成,防护层2003为聚甲基丙烯酸甲酯层b,防护层2003的硬度高、耐磨性好。又或者,防护层2003可以由聚碳酸酯和聚甲基丙烯酸甲酯复合而成,防护层2003为由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,防护层2003既具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性。此处不再赘述。
示例性的,当防护层2003为由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板时,也可以将聚碳酸酯层a和聚甲基丙烯酸甲酯层b经过共挤,挤压成型为复合板而作为防护层2003。这样,防护层2003的层与层之间无需使用粘合剂,防护层2003的整体性好、结构强度高,且不存在溶剂残留问题,此处不再赘述。
另外,由于防护层2003位于醋酸纤维膜2002背离基体2001的一侧,防护层2003远离壳体200的外表面。因而,对防护层2003的表面性能没有特殊要求。当防护层2003为由聚碳酸酯层a和聚甲基丙烯酸甲酯层b复合而成的复合板时,对聚碳酸酯层a和聚甲基丙烯酸甲酯层b叠放位置不作限定。
通过将聚碳酸酯层a、聚甲基丙烯酸甲酯层b或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板作为基体2001和防护层2003,基体2001和防护层2003均采用塑料制作而成。在保证了基体2001和防护层2003的结构强度的基础上,基体2001和防护层2003的成本较低。从而,可以降低壳体200的制作成本,节省电子设备10整机的生产成本。
其中,基体2001的厚度范围可以为0.30mm-0.45mm,或者说,基体2001的厚度可以在0.30mm-0.45mm之间。这样,基体2001具有足够的厚度,以满足基体2001的结构强度需求。进而,保证壳体200具有足够的结构强度,保证壳体200的稳定性和可靠性,保障壳体200的使用寿命。同时,基体2001的厚度也不至于过大,可以减小壳体200的整体厚度,有利于电子设备10的轻薄化。
另外,当基体2001为由聚碳酸酯层a和聚甲基丙烯酸甲酯层b复合而成的复合板时,通过将基体2001的厚度控制在0.30mm-0.45mm之间,不会对单个聚碳酸酯层a和单个聚甲基丙烯酸甲酯层b的厚度造成过多限制,可以保证聚碳酸酯层a和聚甲基丙烯酸甲酯层b稳定性和可靠性。
示例性的,基体2001的厚度可以为0.31mm、0.32mm、0.33mm、0.34mm、0.35mm、0.36mm、0.37mm、0.38mm、0.39mm、0.40mm、0.41mm、0.42mm、0.43mm、0.44mm等。
防护层2003的厚度范围可以为0.05mm-0.15mm,或者说,防护层2003的厚度可以在0.05mm-0.15mm之间。这样,作为设置在醋酸纤维膜2002背离基体2001的一侧的结构层,防护层2003的厚度不至于过小,防护层2003具有足够的结构强度和稳定性,能够起到支撑醋酸纤维膜2002,防止外界水汽进入醋酸纤维膜2002的作用。同时,防护层2003的厚度小于基体2001的厚度,在利用防护层2003提升壳体200的结构强度的基础上,防护层2003的厚度较小,可以减薄壳体200的整体厚度,有利于电子设备10的轻薄化。
另外,当防护层2003为由聚碳酸酯层a和聚甲基丙烯酸甲酯层b复合而成的复合板时,通过将防护层2003的厚度控制在0.05mm-0.15mm之间,不会对单个聚碳酸酯层a和单个聚甲基丙烯酸甲酯层b的厚度造成过多限制,可以保证聚碳酸酯层a和聚甲基丙烯酸甲酯层b稳定性和可靠性。
示例性的,防护层2003的厚度可以为0.06mm、0.07mm、0.08mm、0.09mm、0.10mm、0.11mm、0.12mm、0.13mm、0.14mm等。
醋酸纤维膜2002的厚度范围可以为0.05mm-0.15mm,或者说,醋酸纤维膜2002的厚度可以在0.05mm-0.15mm之间。这样,醋酸纤维膜2002具有一定的厚度,可以保证醋酸纤维膜2002的结构强度和稳定性,保证醋酸纤维膜2002具有良好的纹理效果和光泽度,避免醋酸纤维膜2002背离基体2001的一侧设置的结构层对壳体200的外观效果造成影响。并且,醋酸纤维膜2002的厚度较小,对于变形能力强、结构强度小的醋酸纤维膜2002而言,可以避免醋酸纤维膜2002过厚而影响壳体200的结构强度,保证壳体200的稳定性和可靠性。
示例性的,醋酸纤维膜2002的厚度可以为0.06mm、0.07mm、0.08mm、0.09mm、0.10mm、0.11mm、0.12mm、0.13mm、0.14mm等。
参照图7所示,图中示例出了基体2001为由一层聚碳酸酯层a和一层聚甲基丙烯酸甲酯层b复合而成复合板,聚甲基丙烯酸甲酯层b位于基体2001的外表面所在的一侧,聚碳酸酯层a位于基体2001的内表面所在的一侧。并且,图中示例出了防护层2003为聚碳酸酯层a。
这样,基体2001同时具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性。同时,防护层2003采用单层聚碳酸酯层a,便于加工厚度较薄的防护层2003,且防护层2003具有聚碳酸酯的冲击韧性。从而,可以提升壳体200的可靠性和使用寿命。
参照图8所示,图中示例出了基体2001为由一层聚碳酸酯层a和一层聚甲基丙烯酸甲酯层b复合而成复合板,聚甲基丙烯酸甲酯层b位于基体2001的外表面所在的一侧,聚碳酸酯层a位于基体2001的内表面所在的一侧。并且,图中示例出了防护层2003为由一层聚碳酸酯层a和一层聚甲基丙烯酸甲酯层b复合而成复合板。
这样,基体2001同时具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性。与之类似的,防护层2003同时具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性。从而,可以提升壳体200的可靠性和使用寿命。
参照图9所示,图中示例出了基体2001为聚碳酸酯层a,且图中示例出了防护层2003也为聚碳酸酯层a。这样,基体2001和防护层2003均具有聚碳酸酯的冲击韧性。并且,基体2001和防护层2003均采用单层聚碳酸酯层a,便于基体2001和防护层2003的加工,有利于提高壳体200的制作效率。
参照图10所示,图中示例出了基体2001为聚碳酸酯层a。并且,图中示例出了防护层2003为由一层聚碳酸酯层a和一层聚甲基丙烯酸甲酯层b复合而成复合板。其中,图中示例出的防护层2003,聚碳酸酯层a位于防护层2003朝向醋酸纤维膜2002的一侧,聚甲基丙烯酸甲酯层b位于防护层2003背离醋酸纤维膜2002的一侧。
这样,基体2001具有聚碳酸酯的冲击韧性。并且,基体2001采用单层聚碳酸酯层a,便于基体2001的加工。防护层2003同时具有聚碳酸酯的冲击韧性,又具有聚甲基丙烯酸甲酯的高硬度和耐磨性。从而,可以提升壳体200的可靠性和使用寿命。
参照图7至图10任一所示,由于基体2001和防护层2003均为硬度较高、刚度较大的薄板件,而醋酸纤维膜2002为弹性较好、形变能力较强的薄膜,为了将基体2001、醋酸纤维膜2002及防护层2003三者连接在一起,可以通过粘合剂将基体2001和防护层2003分别粘接在醋酸纤维膜2002的两侧,以实现三者的紧密连接,保证壳体200的整体性和稳定性。
其中,基体2001和醋酸纤维膜2002之间可以设置有第一胶层2004,基体2001和醋酸纤维膜2002通过第一胶层2004粘接在一起。防护层2003和醋酸纤维膜2002之间设置有第二胶层2005,防护层2003和醋酸纤维膜2002通过第二胶层2005粘接在一起。利用第一胶层2004和第二胶层2005,将基体2001和防护层2003牢牢的粘接在醋酸纤维膜2002的两侧,保证三者之间的连接强度。
通过第一胶层2004和第二胶层2005将醋酸纤维膜2002夹住,减少了醋酸纤维膜2002两侧的空隙,保证醋酸纤维膜2002两侧的密实度。并且,醋酸纤维膜2002两侧的基体2001和防护层2003均为高密度的结构件,可以对醋酸纤维膜2002形成良好保护。如此,可以阻止外界水汽从壳体200的两侧及壳体200的侧壁进入醋酸纤维膜2002,避免对醋酸纤维膜2002的纹理效果和光泽度造成影响,保证壳体200的外观效果。
示例性的,第一胶层2004和第二胶层2005中的至少一者为UV胶层。UV(Ultraviolet Rays,紫外线)胶又称紫外光固化胶、光敏胶、无影胶,它是指必须通过紫外光照射才能固化的一类胶粘剂。UV胶的固化方式简单、固化速度快且成本低,采用UV胶将基体2001和防护层2003中的至少一者与醋酸纤维膜2002粘接,可以提升壳体200的制作效率,降低壳体200的制作成本。从而,有利于降低电子设备10整机的生产成本。
例如,基体2001和醋酸纤维膜2002之间的第一胶层2004为UV胶层,防护层2003和醋酸纤维膜2002之间的第二胶层2005也为UV胶层。或者,基体2001和醋酸纤维膜2002之间的第一胶层2004为UV胶层,防护层2003和醋酸纤维膜2002之间的第二胶层2005为其他类型的胶层。又或者,基体2001和醋酸纤维膜2002之间的第一胶层2004为其他类型的胶层,防护层2003和醋酸纤维膜2002之间的第二胶层2005为UV胶层。当然,基体2001和醋酸纤维膜2002之间的第一胶层2004、防护层2003和醋酸纤维膜2002之间的第二胶层2005也可以都为其他类型的胶层。
当第一胶层2004和第二胶层2005中的至少一者选用其他类型的胶层时,该胶层可以为OCA胶层。OCA(Optically Clear Adhesive,光学透明胶粘剂)的透光度高、黏着力高,耐候性、耐水性、耐高温、抗紫外线等能力均较好。采用OCA胶将基体2001和防护层2003中的至少一者与醋酸纤维膜2002连接,可以保证三者之间的粘接强度,保证壳体200的整体性和结构强度。
继续参照图7至图10任一所示,壳体200还包括盖底层2006,盖底层2006设置在防护层2003背离醋酸纤维膜2002的一侧。盖底层2006可以位于壳体200朝向电子设备10内的一侧表面,或者说,盖底层2006作为壳体200的内表层。盖底层2006通常包括多层油墨层,通过在壳体200的内表面印刷或喷涂多层油墨层,可以对壳体200进行保护,防止盖底层2006之下的结构层被磨损或刮花。
盖底层2006相当于壳体200的底漆层,对于盖底层2006包括的多层油墨层,该多层油墨层可以包括位于壳体200表层的一层油墨层和其上印刷的多层油墨层,位于表层的油墨层可以为白色油墨层、灰色油墨层或黑色油墨层,其他油墨层均可以为白色油墨层。以为壳体200提供一个颜色均匀、不透光的底漆层,可以保证壳体200的外观效果。避免采用彩色油墨层作为盖底层2006,以防对壳体200的其他结构层的颜色和质感造成影响,防止对壳体200的外观效果造成影响。
示例性的,盖底层2006可以包括阻燃油墨层,阻燃油墨可以是在油墨中加入阻燃剂,以提升油墨层的阻燃性能。如此,可以防止壳体200意外起火,提升壳体200的安全性和可靠性。
继续参照图7至图10任一所示,壳体200还可以包括强化层2007,强化层2007设置在基体2001的外表面。强化层2007可以位于壳体200朝向电子设备10外的一侧表面,或者说,强化层2007作为壳体200的外表层。强化层2007主要用于对壳体200的外表面进行加硬处理,以增强壳体200的硬度和耐磨性。从而,提升壳体200的稳定性和可靠性,延长壳体200的使用寿命。示例性的,可以采用淋涂或UV转印技术在基体2001的外表面形成一层UV胶层,该UV胶层固化后即作为强化层2007。
并且,还可以在强化层2007朝向基体2001的一侧表面或基体2001的任一侧表面(基体2001的外表面或基体2001的内表面)形成丝印纹理,该丝印纹理例如为电子设备10的标志图案。或者,也可以采用激光刻蚀工艺在基体2001的任一侧表面形成刻蚀纹理,该刻蚀纹理例如为电子设备10的标志图案。
图11为本申请实施例提供的第五种壳体的结构示意图。参照图11所示,图中以基体2001为复合板、防护层2003为聚碳酸酯层a为例。在一些实施方式中,还可以在盖底层2006和防护层2003之间设置其他膜层,以增强壳体200的结构强度和硬度,提升壳体200的可靠性,延长壳体200的使用寿命。
其中,盖底层2006和防护层2003之间可以设置有至少一层镀膜层2008,通过镀膜层2008的加入,提升壳体200的性能。例如,可以增强壳体200的硬度,提升壳体200的抗摔能力,提升壳体200的抗氧化性、耐久性等。
示例性的,设置在盖底层2006和防护层2003之间的镀膜层2008可以包括氧化硅层20081,氧化硅层20081例如附着于盖底层2006。氧化硅(SiO2)为制造玻璃、陶瓷的主要材料,其稳定性好、强度高、硬度高、耐磨性和抗老化性能好。通过在壳体200中加入氧化硅层20081,可以提高壳体200的强度和硬度,增强壳体200的耐磨性能和抗老化性能,还可以防止壳体200进水,也有助于提升壳体200的阻燃性能。从而,可以提升壳体200的稳定性和可靠性,延长壳体200的使用寿命。
在盖底层2006和防护层2003之间设置氧化硅层20081的基础上,还可以在盖底层2006和防护层2003之间加入氧化锆层20082,氧化锆层20082可以设置在氧化硅层20081和防护层2003之间。氧化锆(ZrO2)属于陶瓷材料,其具有电、磁、热、光学等性能,氧化锆具有硬度高、介电常数高、稳定性好、耐腐蚀、抗氧化等优点。通过在壳体200中加入氧化锆层20082,可以使壳体200更加坚固耐磨、不屏蔽信号、散热性好,可以提升壳体200的可靠性和使用寿命。
氧化硅层20081和氧化锆层20082之间可以设置油墨层2009,通过油墨层2009对氧化硅层20081和氧化锆层20082进行隔离。避免在形成氧化锆层20082和氧化硅层20081的过程中,互相影响和互相干扰,保证氧化硅层20081和氧化锆层20082的性能。
继续参照图11,壳体200中还可以设置有UV纹理层2010,UV纹理层2010可以设置在防护层2003和镀膜层2008之间。例如,UV纹理层2010可以形成在防护层2003上。可以通过在模具上加工形成所需纹理,将UV胶滴加在模具上,然后将防护层2003覆盖在模具上,经过辊压、光固化等工序后,将防护层2003从模具上剥离。这样,便可以将模具上的纹理通过UV胶完全复制到防护层2003上,从而实现UV转印,形成UV纹理层2010。
通过在防护层2003和镀膜层2008之间设置UV纹理层2010,在防护层2003上形成UV纹理,可以增强镀膜层2008与防护层2003之间的附着力,提升壳体200的整体性和可靠性。在有些情况下,UV纹理层2010的纹理效果可以透过防护层2003与醋酸纤维膜2002的纹理效果叠加,以提升壳体200的外观效果。
本申请实施例还提供一种电子设备10的壳体200的制作方法(以下简称制作方法),该制作方法用于制作前述电子设备10的壳体200。以下对该制作方法进行详细说明。
图12为本申请实施例提供的壳体的制作方法的步骤流程图。参照图12所示,该制作方法包括如下步骤:
S100、提供基体2001和醋酸纤维膜2002,并将基体2001的内表面和醋酸纤维膜2002贴合连接。
结合图7-图11任一所示,首先,提供基体2001和醋酸纤维膜2002,将基体2001和醋酸纤维膜2002两者叠置并精准对位。然后,将基体2001和醋酸纤维膜2002贴合连接,将两者连接为一个整体。
其中,可以先制作形成醋酸纤维膜2002。以下对醋酸纤维膜2002的制作流程,进行说明。
如前所述,可以先提供粉末状原料。该粉末状原料可以仅包括醋酸纤维原料。或者,也可以在醋酸纤维原料中加入天然矿物粉,两者混合成为粉末状原料。将不同颜色的色粉与粉末状原料混合,形成至少两种不同颜色的粉末状配料。以下以醋酸纤维膜2002由两种颜色的粉末状配料形成,具体以该两种颜色的粉末状配料分别为A配料和B配料为例,进行说明。
形成A配料和B配料之后,将A配料和B配料分别加入溶剂中,对A配料和B配料进行充分揉捏(该过程可以在揉捏机中进行),将A配料和B配料均揉捏均匀,形成质地柔软、体积较大的A块料和B块料。确保A块料和B块料上色均匀,并静置一段时间。
然后,对A块料和B块料进行切割处理,将大块状的A块料和B块料切割成尺寸较大、厚度较薄的薄片状,形成的A大片料和B大片料。再对A大片料和B大片料进行进一步切割处理,将尺寸较大的A大片料和B大片料切割成尺寸较小的小薄片,形成A小片料和B小片料。根据醋酸纤维膜2002的成型需求,还会对呈小薄片状的A小片料和B小片料进行进一步处理,将A小片料和B小片料经挤压和切割等工序成为颗粒状或短柱状,形成A颗粒和B颗粒。例如,A颗粒和B颗粒的长度均为25mm左右。
将A颗粒和B颗粒晾干后,进行下一步混料处理。根据醋酸纤维膜2002的纹理需求,可以将A颗粒和B颗粒混合均匀,或者,将A颗粒和B颗粒进行特定造型的摆放。例如,将A颗粒和B颗粒由中心向外侧交替设置,使醋酸纤维膜2002形成放射状的纹理效果。之后,对摆放好的A颗粒和B颗粒进行加热、加压,形成平面尺寸较大、厚度较大的醋酸纤维板。对醋酸纤维板进行晾干、烘烤和校平,形成干燥、平整的醋酸纤维板。
接下来,对醋酸纤维板进行拉伸处理,可以对醋酸纤维板进行至少一次横向拉伸和至少一次纵向拉伸。在此过程中,尺寸较大、厚度较大的醋酸纤维板被拉伸成为尺寸更大、厚度变薄的醋酸纤维薄片,同时,随着醋酸纤维板的厚度不断减薄,醋酸纤维板上的纹理也不断发生变化,最终的醋酸纤维薄片上呈现壳体200的外观纹理。最后,对醋酸纤维薄片进行裁切,形成尺寸符合要求的醋酸纤维膜2002。
以A颗粒为白色颗粒、B颗粒为浅灰色颗粒为例,将A颗粒和B颗粒混合均匀、热压、拉伸和裁切之后形成的醋酸纤维膜2002,可以具有白色和浅灰色相间的多个色块,且各白色色块和浅灰色色块纹理独特,可以赋予壳体200独特的自然纹理和光泽。
至于基体2001和醋酸纤维膜2002的贴合连接,可以在基体2001和醋酸纤维膜2002中的一者的表面上形成第一胶层2004,将基体2001和醋酸纤维膜2002中的另一者放置在第一胶层2004上,将基体2001和醋酸纤维膜2002对位精准。然后,对基体2001和醋酸纤维膜2002进行压合,以利用第一胶层2004将基体2001和醋酸纤维膜2002粘接在一起,保证基体2001和醋酸纤维膜2002连接牢靠、平整。
可以采用点胶工艺,在基体2001的表面或醋酸纤维膜2002的表面涂覆UV胶或OCA(光学透明胶粘剂),以形成第一胶层2004。其中,当第一胶层2004为UV胶层时,在基体2001或醋酸纤维膜2002上涂覆UV胶之后,需要通过紫外灯对第一胶层2004进行照射,利用紫外灯发出的紫外光,将第一胶层2004固化。并且,可以对紫外灯发出的紫外光的传播方向进行选择,以确保紫外光将第一胶层2004固化完全,保证基体2001和醋酸纤维膜2002连接牢靠。
当基体2001为前述的聚碳酸酯层a时,基体2001对紫外光具有很高的透过率。此时,可以将紫外灯设置在基体2001所在的一侧,紫外灯发出的紫外光穿过基体2001到达第一胶层2004。或者,也可以将紫外灯设置在醋酸纤维膜2002所在的一侧,紫外灯发出的紫外光穿过醋酸纤维膜2002到达第一胶层2004。无论紫外光穿过基体2001到达第一胶层2004,还是紫外光穿过醋酸纤维膜2002到达第一胶层2004,第一胶层2004对紫外光的吸收率均很高,可以保证第一胶层2004固化完全。
当基体2001为前述的聚甲基丙烯酸甲酯层b或复合板时,相较于基体2001,醋酸纤维膜2002对紫外光的透过率更高。此时,可以将紫外灯设置在醋酸纤维膜2002所在的一侧,紫外灯发出的紫外光穿过醋酸纤维膜2002到达第一胶层2004。以确保第一胶层2004对紫外光的吸收率,保证第一胶层2004固化完全。
S200、提供防护层2003,并将防护层2003贴合在醋酸纤维膜2002背离基体2001的一侧表面。
将基体2001和醋酸纤维膜2002通过第一胶层2004粘接在一起之后,接下来,将防护层2003放置在醋酸纤维膜2002背离基体2001的一侧。将防护层2003与醋酸纤维膜2002精准对位,并将防护层2003与醋酸纤维膜2002贴合连接,使基体2001、醋酸纤维膜2002及防护层2003三者贴合在一起。
具体的,可以在防护层2003和醋酸纤维膜2002中的一者的表面上形成第二胶层2005,将醋酸纤维膜2002与基体2001形成的整体和防护层2003中的另一者放置在第二胶层2005上,将防护层2003与醋酸纤维膜2002对位精准后。对基体2001、醋酸纤维膜2002及防护层2003整体进行压合,以利用第二胶层2005将防护层2003和醋酸纤维膜2002粘接在一起,保证防护层2003与醋酸纤维膜2002连接牢靠、平整。
类似的,也可以采用点胶工艺在防护层2003的表面或醋酸纤维膜2002的表面涂覆UV胶或OCA(光学透明胶粘剂),以形成第二胶层2005。其中,当第二胶层2005为UV胶层时,通过紫外灯照射第一胶层2004,利用紫外灯发出的紫外光将第二胶层2005进行固化。同样的,也可以对紫外灯发出的紫外光的传播方向进行选择,以保证紫外光将第二胶层2005固化完全,保证防护层2003和醋酸纤维膜2002连接牢靠。
当基体2001和防护层2003均为前述的聚碳酸酯层a时,基体2001和防护层2003对紫外光均具有很高的透过率。此时,可以将紫外灯设置在防护层2003所在的一侧,以使紫外灯发出的紫外光穿过防护层2003到达第二胶层2005。或者,也可以将紫外灯设置在基体2001所在的一侧,紫外灯发出的紫外光依次穿过基体2001、第一胶层2004及醋酸纤维膜2002到达第二胶层2005。由于防护层2003、基体2001及第一胶层2004的透光度均很高,因此,无论紫外灯如何设置,第二胶层2005对紫外光的吸收效率均很高,可以保证第二胶层2005完全固化。其中,当紫外灯设置在防护层2003所在的一侧时,紫外光穿透的结构层较少,第二胶层2005对紫外光的吸收速率快,第二胶层2005的固化速率高。
当防护层2003为前述的聚碳酸酯层a、基体2001为前述的聚甲基丙烯酸甲酯层b或合板时,相较于基体2001,防护层2003对紫外光的透过率更高。此时,可以将紫外灯设置在防护层2003所在的一侧,紫外光穿过防护层2003到达第二胶层2005。相反的,当基体2001为前述的聚碳酸酯层a、防护层2003为前述的聚甲基丙烯酸甲酯层b或复合板时,相较于防护层2003,基体2001对紫外光的透过率更高。此时,可以将紫外灯设置在基体2001所在的一侧,紫外光依次穿过基体2001、第一胶层2004及醋酸纤维膜2002到达第二胶层2005。如此设置,可以确保第二胶层2005对紫外光的吸收率,保证第二胶层2005完全固化。
当防护层2003和基体2001均为前述的聚甲基丙烯酸甲酯层b或合板时,防护层2003和基体2001对紫外光的透过率相当。因此,既可以将紫外灯设置在防护层2003所在的一侧,也可以将紫外灯设置在基体2001所在的一侧。可以适当延长紫外灯的照射时间,以确保第二胶层2005完全固化。
结合图7至图11任一所示,当将基体2001、醋酸纤维膜2002及防护层2003贴合在一起之后,可以在防护层2003背离醋酸纤维膜2002的一侧形成盖底层2006,盖底层2006位于壳体200朝向电子设备10内的一侧表面。例如,可以在防护层2003背离醋酸纤维膜2002的一侧,印刷或喷涂多层油墨层作为盖底层2006。
并且,还可以在基体2001的外表面,也就是基体2001背离醋酸纤维膜2002的一侧表面,形成强化层2007。例如,可以通过淋涂或UV转印技术在基体2001的外表面形成一层UV胶层,该UV胶层固化后即作为强化层2007。
结合图11所示,当防护层2003和盖底之间还设置有其他结构层时,在形成盖底层2006之前,可以先在防护层2003上依次形成这些结构层,最后,再将盖底层2006形成在这些结构层上。
示例性的,设置在防护层2003和盖底之间的结构层可以包括至少一层镀膜层2008。可以先在防护层2003背离醋酸纤维膜2002的一侧形成镀膜层2008,之后,再将盖底形成在镀膜层2008上。以镀膜层2008包括氧化硅层20081和氧化锆层20082为例,可以先在防护层2003背离醋酸纤维膜2002的一侧形成氧化锆层20082,再在氧化锆层20082背离防护层2003的一侧形成氧化硅层20081。其中,可以在形成氧化硅层20081之前,在氧化锆层20082上印刷或喷涂一层油墨层2009,再在油墨层2009上形成氧化硅层20081。
在此基础上,设置在防护层2003和盖底之间的结构层还可以包括UV纹理层2010,UV纹理层2010可以设置在防护层2003和镀膜层2008之间。此时,在防护层2003背离醋酸纤维膜2002的一侧形成镀膜层2008之前,可以先通过UV转印工艺在防护层2003上形成UV纹理层2010,再将镀膜层2008形成在UV纹理层2010上。
在本申请实施例的描述中,需要说明的是,除非另有明确的规定和限定,术语“安装”、“相连”、“连接”应作广义理解,例如,可以是固定连接,也可以是通过中间媒介间接相连,可以是两个元件内部的连通或者两个元件的相互作用关系。对于本领域的普通技术人员而言,可以根据具体情况理解上述术语在本申请实施例中的具体含义。
本申请实施例的说明书和权利要求书及上述附图中的术语“第一”、“第二”、“第三”、“第四”等(如果存在)是用于区别类似的对象,而不必用于描述特定的顺序或先后次序。
Claims (21)
- 一种电子设备的壳体,其特征在于,包括:基体,包括相对设置的外表面和内表面;所述基体为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板;醋酸纤维膜,设置在所述基体的内表面所在的一侧;防护层,设置在所述醋酸纤维膜背离所述基体的一侧;所述防护层为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板。
- 根据权利要求1所述的电子设备的壳体,其特征在于,所述基体和所述醋酸纤维膜之间设置有第一胶层,所述防护层和所述醋酸纤维膜之间设置有第二胶层。
- 根据权利要求2所述的电子设备的壳体,其特征在于,所述第一胶层和所述第二胶层中的至少一者为UV胶层。
- 根据权利要求1-3任一项所述的电子设备的壳体,其特征在于,所述基体的厚度范围为0.30mm-0.45mm,所述防护层的厚度范围为0.05mm-0.15mm。
- 根据权利要求1-3任一项所述的电子设备的壳体,其特征在于,所述醋酸纤维膜的厚度范围为0.05mm-0.15mm。
- 根据权利要求1-3任一项所述的电子设备的壳体,其特征在于,还包括:盖底层,设置在所述防护层背离所述醋酸纤维膜的一侧。
- 根据权利要求6所述的电子设备的壳体,其特征在于,还包括:至少一层镀膜层,设置在所述盖底层和所述防护层之间。
- 根据权利要求7所述的电子设备的壳体,其特征在于,至少一层所述镀膜层包括:氧化硅层,附着于所述盖底层;氧化锆层,设置于所述氧化硅层和所述防护层之间。
- 根据权利要求8所述的电子设备的壳体,其特征在于,所述氧化硅层和所述氧化锆层之间设置有油墨层。
- 根据权利要求7所述的电子设备的壳体,其特征在于,还包括:UV纹理层,设置在所述防护层和所述镀膜层之间。
- 根据权利要求1-3任一项所述的电子设备的壳体,其特征在于,还包括:强化层,设置在所述基体的外表面。
- 一种电子设备的壳体的制作方法,其特征在于,包括:提供基体和醋酸纤维膜,并将所述基体的内表面和所述醋酸纤维膜贴合连接;提供防护层,并将防护层贴合在所述醋酸纤维膜背离所述基体的一侧表面;其中,所述基体和所述防护层分别为聚碳酸酯层、聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板。
- 根据权利要求12所述的电子设备的壳体的制作方法,其特征在于,将所述基体和所述醋酸纤维膜贴合连接,包括:在所述基体和所述醋酸纤维膜中的一者的表面上形成第一胶层;将所述基体和所述醋酸纤维膜通过所述第一胶层贴合连接;和/或,将所述防护层贴合在所述醋酸纤维膜背离所述基体的一侧表面,包括:在所述醋酸纤维膜背离所述基体的一侧表面上形成第二胶层;将所述防护层通过所述第二胶层贴合在所述醋酸纤维膜背离所述基体的一侧表面。
- 根据权利要求13所述的电子设备的壳体的制作方法,其特征在于,当所述基体为聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,且所述第一胶层为UV胶层时,将所述基体和所述醋酸纤维膜通过所述第一胶层贴合连接,包括:将紫外灯设置在所述醋酸纤维膜所在的一侧,使所述紫外灯发出的紫外光穿过所述醋酸纤维膜到达所述第一胶层,以将所述第一胶层固化。
- 根据权利要求13所述的电子设备的壳体的制作方法,其特征在于,当所述防护层为聚碳酸酯层,且所述第二胶层为UV胶层时,将所述防护层贴合在所述醋酸纤维膜背离所述基体的一侧表面,包括:将紫外灯设置在所述防护层所在的一侧,使所述紫外灯发出的紫外光穿过所述防护层到达所述第二胶层,以将所述第二胶层固化。
- 根据权利要求13所述的电子设备的壳体的制作方法,其特征在于,当所述基体为聚碳酸酯层,所述防护层为聚甲基丙烯酸甲酯层或由聚碳酸酯和聚甲基丙烯酸甲酯复合而成的复合板,且所述第二胶层为UV胶层时,将所述防护层贴合在所述醋酸纤维膜背离所述基体的一侧表面,包括:将紫外灯设置在所述基体所在的一侧,使所述紫外灯发出的紫外光依次穿过所述基体、所述第一胶层及所述醋酸纤维膜到达所述第二胶层,以将所述第二胶层固化。
- 根据权利要求12-16任一项所述的电子设备的壳体的制作方法,其特征在于,还包括:在所述防护层背离所述醋酸纤维膜的一侧形成盖底层。
- 根据权利要求17所述的电子设备的壳体的制作方法,其特征在于,还包括:在所述盖底层和所述防护层之间形成至少一层镀膜层。
- 根据权利要求18所述的电子设备的壳体的制作方法,其特征在于,还包括:在所述防护层和所述镀膜层之间形成UV纹理层。
- 根据权利要求12-16任一项所述的电子设备的壳体的制作方法,其特征在于,还包括:在所述基体的外表面形成强化层。
- 一种电子设备,其特征在于,包括显示屏和权利要求1-11任一项所述的壳体,所述显示屏安装于所述壳体。