WO2024075388A1 - 発光素子および発光素子の製造方法 - Google Patents
発光素子および発光素子の製造方法 Download PDFInfo
- Publication number
- WO2024075388A1 WO2024075388A1 PCT/JP2023/028862 JP2023028862W WO2024075388A1 WO 2024075388 A1 WO2024075388 A1 WO 2024075388A1 JP 2023028862 W JP2023028862 W JP 2023028862W WO 2024075388 A1 WO2024075388 A1 WO 2024075388A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- buffer layer
- gallium nitride
- substrate
- light
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10H—INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- H10H20/00—Individual inorganic light-emitting semiconductor devices having potential barriers, e.g. light-emitting diodes [LED]
- H10H20/80—Constructional details
- H10H20/81—Bodies
- H10H20/822—Materials of the light-emitting regions
- H10H20/824—Materials of the light-emitting regions comprising only Group III-V materials, e.g. GaP
- H10H20/825—Materials of the light-emitting regions comprising only Group III-V materials, e.g. GaP containing nitrogen, e.g. GaN
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10H—INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- H10H20/00—Individual inorganic light-emitting semiconductor devices having potential barriers, e.g. light-emitting diodes [LED]
- H10H20/01—Manufacture or treatment
- H10H20/011—Manufacture or treatment of bodies, e.g. forming semiconductor layers
- H10H20/013—Manufacture or treatment of bodies, e.g. forming semiconductor layers having light-emitting regions comprising only Group III-V materials
- H10H20/0133—Manufacture or treatment of bodies, e.g. forming semiconductor layers having light-emitting regions comprising only Group III-V materials with a substrate not being Group III-V materials
- H10H20/01335—Manufacture or treatment of bodies, e.g. forming semiconductor layers having light-emitting regions comprising only Group III-V materials with a substrate not being Group III-V materials the light-emitting regions comprising nitride materials
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10H—INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- H10H20/00—Individual inorganic light-emitting semiconductor devices having potential barriers, e.g. light-emitting diodes [LED]
- H10H20/80—Constructional details
- H10H20/81—Bodies
- H10H20/815—Bodies having stress relaxation structures, e.g. buffer layers
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
- H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
Definitions
- One embodiment of the present invention relates to a semiconductor element, such as a light-emitting element or a transistor, and a method for manufacturing the same.
- a semiconductor element such as a light-emitting element or a transistor
- a method for manufacturing the same for example, one embodiment of the present invention relates to a semiconductor element including a gallium nitride semiconductor and a method for manufacturing the same.
- Typical examples of semiconductor elements include light-emitting elements and transistors.
- semiconductor elements that contain nitrides of group 13 elements, such as gallium nitride (GaN) and indium nitride (InN).
- GaN gallium nitride
- InN indium nitride
- Patent Documents 1 to 3 disclose that light-emitting elements and transistors having semiconductor layers that contain nitrides of group 13 elements can be formed on glass substrates.
- An object of one embodiment of the present invention is to provide a semiconductor element having a novel structure and a method for manufacturing the same.
- an object of one embodiment of the present invention is to provide a light-emitting element or transistor that contains a group 13 element and a group 15 element in the semiconductor layer and a method for manufacturing the same.
- the light-emitting device includes a substrate including amorphous glass, a first buffer layer, a second buffer layer, a gallium nitride layer, a stack, and a cathode and an anode.
- the first buffer layer is located on the substrate and includes aluminum and oxygen.
- the second buffer layer is located on the first buffer layer and includes aluminum and nitrogen.
- the gallium nitride layer is located on the second buffer layer.
- the stack is located on the gallium nitride layer and includes an n-type cladding layer, a p-type cladding layer, and a light-emitting layer between the n-type cladding layer and the p-type cladding layer.
- the cathode and the anode are located on the n-type cladding layer and the p-type cladding layer, respectively.
- the n-type cladding layer, the p-type cladding layer, and the light-emitting layer each include a Group 13 element and a Group 15 element.
- One embodiment of the present invention is a method for manufacturing a light-emitting device.
- the method includes forming a first buffer layer on a substrate containing amorphous glass, forming a second buffer layer on the first buffer layer, forming a gallium nitride layer on the second buffer layer by a sputtering method, forming a laminate including an n-type cladding layer, a p-type cladding layer, and a light-emitting layer between the n-type cladding layer and the p-type cladding layer on the gallium nitride layer by a sputtering method, and forming a cathode and an anode on each of the n-type cladding layer and the p-type cladding layer, wherein each of the n-type cladding layer, the p-type cladding layer, and the light-emitting layer includes a group 13 element and a group 15 element.
- One embodiment of the present invention is a display device that includes a plurality of the above-described light-emitting elements.
- One embodiment of the present invention is a transistor.
- the transistor includes a substrate containing amorphous glass, a first buffer layer, a second buffer layer, an active layer containing a group 13 element and a group 15 element, a gate insulating film, a gate electrode, and a first terminal and a second terminal.
- the first buffer layer is located on the substrate, and the second buffer layer is located on the first buffer layer.
- the active layer is located on the second buffer layer, and the gate insulating film is located on the active layer.
- the first terminal and the second terminal are located on the active layer and are in contact with the active layer.
- the gate electrode is located on the active layer via the gate insulating film.
- FIG. 1 is a schematic end view of a light-emitting device according to an embodiment of the present invention.
- FIG. 1 is a schematic end view of a light-emitting device according to an embodiment of the present invention.
- 4 is a graph showing the relationship of lattice constants of components included in a light-emitting device according to an embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- 5A to 5C are schematic end views illustrating a method for manufacturing a light-emitting device according to one embodiment of the present invention.
- FIG. 1 is a schematic end view of a transistor according to an embodiment of the present invention.
- FIG. 1 is a schematic end view of a transistor according to an embodiment of the present invention.
- the term "on top” is used, unless otherwise specified, to include both a case in which another structure is placed directly on top of a structure so as to be in contact with the structure, and a case in which another structure is placed above a structure via yet another structure.
- a structure exposed from another structure refers to a configuration in which a portion of a structure is not covered by another structure, and includes a configuration in which the portion not covered by the other structure is covered by yet another structure.
- the configuration expressed by this expression also includes a configuration in which a structure is not in contact with the other structure.
- the light-emitting device is an inorganic light-emitting diode (LED) having a semiconductor layer containing a Group 13 element and a Group 15 element.
- LED inorganic light-emitting diode
- FIG. 1A shows a schematic end view of a light-emitting device 100 according to an embodiment of the present invention.
- the light-emitting device 100 has a substrate 102 containing amorphous glass, and two buffer layers (a first buffer layer 110 and a second buffer layer 112) on the substrate 102.
- the light-emitting device 100 further has a gallium nitride layer 120 on the second buffer layer 112 in contact with the second buffer layer 112, and has a laminate on the gallium nitride layer 120 including an n-type cladding layer 122, a p-type cladding layer 126, and a light-emitting layer 124 sandwiched between the n-type cladding layer 122 and the p-type cladding layer 126.
- the light-emitting device 100 further has an anode 128 and a cathode 130 provided on the p-type cladding layer 126 and the gallium nitride layer 120, respectively.
- the first buffer layer 110 may be in direct contact with the substrate 102, or may be provided on the substrate 102 via an overcoat 104 having an arbitrary configuration.
- anode 128 and the cathode 130 that is equal to or greater than the light emission threshold voltage, holes and electrons are injected from the anode 128 and the cathode 130, respectively, and the holes and electrons recombine in the light emitting layer 124, resulting in light emission.
- the light-emitting element 100 may further include a protective film 140 on the anode 128 and the cathode 130.
- the light-emitting element 100 may also include an undercoat 106 under the substrate 102. These configurations are described below.
- the substrate 102 is a component that supports each component provided thereon, and includes amorphous glass.
- a substrate having a high strain point and high surface flatness is used as the substrate 102.
- the substrate 102 preferably has a strain point of 600° C. or higher.
- the substrate 102 may be thick enough to be flexible (e.g., 0.1 mm or more and 0.5 mm or less), or may be thicker than this (e.g., 0.5 mm or more and 2 mm or less).
- the substrate 102 is a glass substrate known as alkali-free glass.
- the substrate 102 contains silicon dioxide, aluminum oxide, boron oxide, and alkaline earth metal oxides such as calcium oxide and barium oxide.
- the content of alkali metals such as sodium in the substrate 102 is preferably 0.1% or less.
- the overcoat 104 which is an optional configuration, is provided on the substrate 102 so as to be in contact with the substrate 102.
- the overcoat 104 has a function of preventing the diffusion of impurities such as trace amounts of alkali metal ions contained in the substrate 102, and is a laminate of one or more films containing silicon-containing inorganic compounds such as silicon oxide and silicon nitride.
- the overcoat 104 is formed, for example, by a sputtering method or a chemical vapor deposition (CVD) method.
- the undercoat 106 which is disposed under the substrate 102 and is provided so as to be in contact with the substrate 102, is a film having a function of suppressing the detachment of water and the like from the substrate 102 under high temperature conditions during the manufacture of the light emitting element 100, and preventing impurities containing oxygen from being mixed into the gallium nitride layer 120 constituting the light emitting element 100 and the semiconductor layers provided thereon, such as the n-type cladding layer 122, the light emitting layer 124, and the p-type cladding layer 126.
- the undercoat 106 has a function of preventing warping of the substrate 102 caused by the difference in thermal expansion coefficient between the substrate 102 and the gallium nitride layer 120.
- the undercoat 106 having such a function is configured so that its thermal expansion coefficient is between that of the substrate 102 and that of the gallium nitride layer 120. Specifically, the undercoat 106 is configured so that its thermal expansion coefficient is higher than 4.0 ⁇ 10 ⁇ 6 /° C. and less than 5.0 ⁇ 10 ⁇ 6 /° C.
- a film containing aluminum nitride, a film containing aluminum oxide, or a laminate of these can be used as the undercoat 106.
- the undercoat 106 may be formed by using a sputtering method or the like.
- the first buffer layer 110 and the second buffer layer 112 are configured to contribute to the promotion of crystallization of the gallium nitride layer 120 provided thereon.
- the first buffer layer 110 and the second buffer layer 112 are films that prevent deformation (warping) of the substrate 102 under high temperature conditions during the manufacture of the light emitting element 100 by improving adhesion with the substrate 102, and prevent peeling and cracking of each layer provided thereon. For this reason, by using the first buffer layer 110 and the second buffer layer 112, it is possible to prevent cracking in the gallium nitride layer 120 and the semiconductor layer provided thereon without deformation of the substrate 102 or peeling of the gallium nitride layer 120, and to improve the crystallinity of these layers.
- the first buffer layer 110 is provided on the substrate 102 directly or via an overcoat 104.
- the first buffer layer 110 includes an inorganic compound containing aluminum and oxygen, specifically, aluminum oxide.
- the first buffer layer 110 may include aluminum oxide (aluminum oxynitride) containing nitrogen in addition to aluminum and oxygen.
- the composition of the first buffer layer 110 can be expressed by Al x O y (Formula 1), where y/x in Formula 1 may be 1.4 or more and 1.6 or less.
- the composition of the first buffer layer 110 can be expressed by Al x O y N z (Formula 2).
- (2y+3z)/3x may be 0.9 or more and 1.1 or less, and z/y may be 0.05 or more and 0.2 or less. Since the first buffer layer 110 contains aluminum oxide or aluminum oxide containing nitrogen, the first buffer layer 110 can form a strong bond with the aluminum oxide contained in the substrate 102 containing amorphous glass. Therefore, peeling between the substrate 102 and the first buffer layer 110 is effectively suppressed.
- the composition of the first buffer layer 110 may be constant in the thickness direction, or the oxygen concentration may decrease as the distance from the substrate 102 increases (i.e., as the oxygen concentration approaches the second buffer layer 112). In this way, by forming the first buffer layer 110 with a low oxygen concentration on the upper surface, the oxygen concentration in the second buffer layer 112 in contact with the first buffer layer 110 can be reduced.
- the surface of the first buffer layer 110 has high flatness.
- the thickness of the first buffer layer 110 is preferably 50 nm or less, and the first buffer layer 110 is formed with a thickness of, for example, 2 nm to 50 nm.
- the second buffer layer 112 is provided on the first buffer layer 110 so as to be in contact with the first buffer layer 110.
- the second buffer layer 112 includes an inorganic compound containing aluminum and nitrogen, such as aluminum nitride.
- the composition of the second buffer layer 112 can be expressed as Al x N y (Formula 3), where x/y may be 0.9 or more and 1.1 or less.
- the second buffer layer 112 may contain oxygen, but the concentration thereof (for example, the average concentration of oxygen in the second buffer layer 112) is lower than that of the first buffer layer 110.
- the composition of the second buffer layer 112 may also be constant in the thickness direction, or the nitrogen concentration may increase or decrease as the distance from the first buffer layer 110 increases (i.e., as the layer approaches the gallium nitride layer 120). Alternatively, the nitrogen concentration may vary in the film thickness direction with increasing distance from the first buffer layer 110 such that the ratio of x to y (x/y) in Equation 3 approaches 1.
- the composition of the second buffer layer 112 is preferably substantially AlN (i.e., x and y are the same or substantially the same).
- the surface of the second buffer layer 112 is also highly flat.
- the second buffer layer 112 can contain aluminum nitride, and therefore can have a hexagonal close-packed structure, a face-centered cubic structure, or a structure equivalent thereto.
- the hexagonal close-packed structure or a structure equivalent thereto includes a crystal structure in which the c-axis is not perpendicular to the a-axis and the b-axis. Therefore, in this structure, the second buffer layer 112 is oriented in the (0001) direction, i.e., the c-axis direction, relative to its surface.
- the second buffer layer 112 having a face-centered cubic structure or a structure equivalent thereto is oriented in the (111) direction relative to its surface.
- the c-axis of the second buffer layer 112 is oriented in a direction perpendicular or approximately perpendicular to the surface on which the second buffer layer 112 is provided (i.e., the upper surface of the first buffer layer 110).
- the second buffer layer 112 and the gallium nitride layer 120, n-type cladding layer 122, light-emitting layer 124, and p-type cladding layer 126 formed thereon contain semiconductors containing group 13 and group 15 elements such as gallium nitride, but gallium nitride has a hexagonal close-packed structure and is known to grow crystals in the c-axis direction so as to minimize its surface energy.
- the gallium nitride layer 120 on the second buffer layer 112
- crystal growth in the c-axis direction of not only the gallium nitride layer 120 but also the semiconductor layer formed thereon is promoted.
- the crystallinity of these layers is improved, and excellent characteristics as a light-emitting element can be obtained.
- thermal expansion coefficients of the first buffer layer and the second buffer layer are both between the thermal expansion coefficient of the substrate 102 and the thermal expansion coefficient of the gallium nitride layer 120.
- the thermal expansion coefficient of the substrate 102 containing amorphous glass is 3.5 ⁇ 10 ⁇ 6 /°C to 3.9 ⁇ 10 ⁇ 6 /°C
- the expansion coefficient of the gallium nitride contained in the gallium nitride layer 120 in the in-plane direction is 5.6 ⁇ 10 ⁇ 6 /°C.
- the thermal expansion coefficient of the first buffer layer 110 in the in-plane direction depends on the composition and is 3.5 ⁇ 10 ⁇ 6 /°C or more and 5.6 ⁇ 10 ⁇ 6 /°C or less.
- the thermal expansion coefficient in the in-plane direction of the second buffer layer 112 also depends on the composition, and is 3.6 ⁇ 10 ⁇ 6 /° C. or more and 4.6 ⁇ 10 ⁇ 6 /° C. or less. Therefore, in the light emitting device 100, the thermal expansion coefficient in the in-plane direction can be changed (increased) stepwise in the direction from the substrate 102 to the gallium nitride layer 120, and there is no large difference in the thermal expansion coefficient between adjacent components. As a result, no large stress is generated under high temperature conditions during the manufacture of the light emitting device 100, and peeling between adjacent components and the generation of cracks in each layer can be effectively prevented.
- the lattice constant is generally not defined, but it can be said that the crystal structure of silicon oxide, which is its main component, determines the crystallinity of the first buffer layer 110 provided on the substrate 102. Therefore, in this specification, the value 0.491 nm calculated from the broad peak of 2 ⁇ in the X-ray diffraction of amorphous glass near 22° is adopted as the lattice constant in the a-axis direction of the substrate 102.
- the lattice constant in the a-axis direction of the gallium nitride contained in the gallium nitride layer 120 is 0.318 nm.
- the lattice constants in the a-axis direction of the first buffer layer 110 and the second buffer layer 112 having the above configuration both depend on the composition, the former being 0.355 nm or more and 0.480 nm or less, and the latter being 0.300 nm or more and 0.330 nm or less.
- the relationship of the lattice constants among the substrate 102, the first buffer layer 110, the second buffer layer 112, and the gallium nitride layer 120 is shown diagrammatically in Fig. 2.
- the lattice constant in the a-axis direction is gradually reduced in the order of the substrate 102, the first buffer layer 110, the second buffer layer 112, and the gallium nitride layer 120.
- the difference in the lattice constants in the a-axis direction between the first buffer layer 110 containing aluminum oxide and the gallium nitride layer 120 containing gallium nitride ( ⁇ 1 ) is smaller than the difference in the lattice constants ( ⁇ 2 ) between the substrate 102 containing amorphous glass and the gallium nitride layer 120.
- the difference in lattice constant in the a-axis direction between the second buffer layer 112 containing aluminum nitride and the gallium nitride layer 120 ( ⁇ 3 ) is smaller than that between the substrate 102 and the gallium nitride layer 120 ( ⁇ 2 ), and is also smaller than that between the first buffer layer 110 and the gallium nitride layer 120 ( ⁇ 1 ).
- the difference ⁇ 3 in the lattice constant in the a-axis direction between the second buffer layer 112 and the gallium nitride layer 120 is small, the crystal structure of the gallium nitride layer 120 formed on the second buffer layer 112 is easily affected by the second buffer layer 112. Therefore, when the second buffer layer 112 is highly c-axis oriented, the crystallization in the c-axis direction of the gallium nitride layer 120 is also effectively promoted, but when the crystallinity of the second buffer layer 112 is low, the gallium nitride layer 120 cannot be sufficiently crystallized, which causes a decrease in the crystallite size.
- the difference ⁇ 2 between the lattice constant of the substrate 102 and the lattice constant of the second buffer layer 112 is large, and when the second buffer layer is formed directly on the substrate 102, the crystal growth of the second buffer layer 112 is hindered due to the large difference in lattice constant.
- the mismatch in the lattice constant between the substrate 102 and the second buffer layer 112 is alleviated, and by forming the second buffer layer 112 on the first buffer layer 110, the crystallization of the second buffer layer 112 can be promoted.
- the second buffer layer 112 having improved crystallinity is obtained, and by forming the gallium nitride layer 120 on this, the crystallinity in the c-axis direction of the gallium nitride layer 120 can be improved. As a result, the crystallinity of the semiconductor layer provided on the gallium nitride layer 120 can also be improved, and a light-emitting element 100 having excellent characteristics can be provided.
- the gallium nitride layer 120 includes gallium nitride.
- Gallium nitride is given p-type or n-type conductivity by adding a dopant, but the gallium nitride layer 120 may be an undoped gallium nitride layer that does not include a dopant.
- the gallium nitride layer 120 may include n-type gallium nitride containing a dopant that imparts n-type conductivity (such as silicon or germanium), or p-type gallium nitride containing a dopant that imparts p-type conductivity (such as magnesium, zinc, cadmium, or beryllium).
- n-type cladding layer, light-emitting layer, p-type cladding layer The n-type cladding layer 122, light-emitting layer 124, and p-type cladding layer 126 are configured to emit visible light by recombining holes and electrons injected from the anode 128 and the cathode 130, respectively.
- the n-type cladding layer 122, light-emitting layer 124, and p-type cladding layer 126 may each have a single-layer structure, or a laminated structure in which multiple layers are laminated. In the example shown in FIG.
- the n-type cladding layer 122, light-emitting layer 124, and p-type cladding layer 126 are laminated in this order from the substrate 102 side, but the semiconductor layers may be configured in the reverse order.
- the gallium nitride layer 120 is configured to contain undoped gallium nitride or p-type gallium nitride, and the p-type cladding layer 126, light-emitting layer 124, and n-type cladding layer 122 are formed thereon.
- the n-type cladding layer 122, the light-emitting layer 124, and the p-type cladding layer 126 are semiconductor layers containing Group 13 elements and Group 15 elements, respectively. Specifically, these layers contain semiconductors containing aluminum, gallium, and/or indium, as well as nitrogen, phosphorus, and/or arsenic. Typical semiconductors include gallium-based materials.
- Examples include gallium nitride-based materials such as gallium nitride, aluminum gallium nitride (AlGaN), and indium gallium nitride (InGaN), and gallium phosphide-based materials such as gallium phosphide (GaP) and aluminum indium gallium phosphide (AlGaInP).
- the n-type cladding layer 122 and the p-type cladding layer 126 may further contain the above-mentioned dopants. By adding a dopant, it is possible to control the valence electrons of each layer and also to control the band gap.
- the gallium nitride layer 120 and the layer provided in contact therewith may have the same composition.
- the light-emitting layer 124 may be, for example, a single-layer structure of indium gallium nitride, or may have a quantum well structure.
- a quantum well structure is a structure in which multiple thin films with different bandgaps and thicknesses of about 1 to 5 nm are alternately stacked. Examples of such structures include an alternating stack of indium gallium nitride and gallium nitride, an alternating stack of indium gallium arsenide phosphide (GaInAsP) and indium phosphide (InP), and an alternating stack of aluminum indium arsenide (AlInAs) and indium gallium arsenide (InGaAs).
- the anode 128 and the cathode 130 inject holes and electrons into the p-type cladding layer 126 and the n-type cladding layer 122, respectively.
- the anode 128 may be made of a metal such as palladium or gold, an alloy thereof, or a thin film of a conductive oxide that transmits visible light, such as indium-tin mixed oxide (ITO) or indium-zinc mixed oxide (IZO).
- the cathode 130 may be made of a metal such as aluminum, titanium, gold, silver, or indium, or an alloy thereof. Both the anode 128 and the cathode 130 may have a single-layer structure, or may be a laminate of multiple films having different compositions.
- the protective film 140 is configured to prevent impurities such as oxygen and water from entering the light-emitting element 100, and is composed of one or more films containing a silicon-containing inorganic compound such as silicon oxide or silicon nitride.
- the protective film 140 has openings for exposing the anode 128 and the cathode 130, and wiring (not shown) is electrically connected to the anode 128 and the cathode 130 by using these openings.
- the first buffer layer 110 and the second buffer layer 112 are laminated on the substrate 102 containing amorphous glass, and the gallium nitride layer 120 is provided on top of them.
- the substrate 102 and the first buffer layer 110 contain aluminum oxide, so that a strong bond is obtained between them.
- the thermal expansion coefficient increases stepwise from the first buffer layer 110 to the gallium nitride layer 120, and there is no large difference in the thermal expansion coefficient between adjacent components, so that peeling and cracking under high temperature conditions can be prevented.
- the first buffer layer 110 having the lattice constant between the substrate 102 and the second buffer layer 112 is provided between the substrate 102 and the second buffer layer 112, which have a large difference in lattice constant, the large lattice mismatch between the substrate 102 and the second buffer layer 112 can be alleviated. Therefore, by providing the second buffer layer 112 on the first buffer layer 110 having a high bonding strength with the substrate 102, the crystallinity of the second buffer layer 112 can be greatly improved compared to the case where the second buffer layer 112 is provided directly on the substrate 102.
- the crystallinity of the n-type cladding layer 122, the light-emitting layer 124, and the p-type cladding layer 126, which determine the function of the light-emitting element 100, is improved, making it possible to provide a light-emitting element with excellent characteristics.
- the aluminum oxide, aluminum oxynitride, and aluminum nitride contained in the first buffer layer 110 and the second buffer layer 112 are highly resistant to various etchants used in photolithography processes, and therefore will not be lost or damaged during the manufacturing process of the light-emitting element 100 described below. Therefore, it is possible to manufacture a highly reliable light-emitting element 100 using various conventional devices for manufacturing semiconductor devices.
- the structure of the light-emitting element 100 is not limited to the above-mentioned structure.
- three or more buffer layers may be provided between the substrate 102 and the gallium nitride layer 120.
- a third buffer layer 114 on the second buffer layer 112 and a fourth buffer layer 116 on the third buffer layer 114 may be provided. Adjacent buffer layers are provided to contact each other.
- the third buffer layer 114 and the fourth buffer layer 116 may have the same configuration as the first buffer layer 110 and the second buffer layer 112, respectively.
- each of the first buffer layer 110 to the fourth buffer layer 116 may contain aluminum oxide, aluminum oxynitride, or aluminum nitride, with the oxygen concentration decreasing and the nitrogen concentration increasing in the order from the first buffer layer 110 to the fourth buffer layer 116.
- the fourth buffer layer 116 contains aluminum nitride.
- the lattice mismatch between the buffer layer in contact with the gallium nitride layer 120 and the substrate 102 is alleviated, and the difference in thermal expansion coefficient between adjacent structures can be reduced.
- a gallium nitride layer 120 with high crystallinity can be formed, and the occurrence of peeling and cracks can be suppressed.
- Second Embodiment In this embodiment, a description will be given of a method for manufacturing the light emitting device 100. Descriptions of configurations that are the same as or similar to the configuration described in the first embodiment may be omitted.
- the overcoat 104 and the undercoat 106 are formed on the top and bottom of the substrate 102, respectively.
- the substrate 102 There is no restriction on the size of the substrate 102, and it is also possible to use a large amorphous glass substrate, also called mother glass, as the substrate 102.
- a large amorphous glass substrate also called mother glass
- an amorphous glass substrate having a size of 600 mm ⁇ 720 mm, called 3.5th generation glass, a size of 730 mm ⁇ 920 mm, called 4.5th generation glass, a size of 1500 mm ⁇ 1850 mm, or a size larger than that, called 6th generation glass may be used. Therefore, a plurality of light-emitting elements 100 can be manufactured using one substrate 102.
- the overcoat 104 and the undercoat 106 may be formed using a CVD method or a sputtering method. Note that the overcoat 104 and the undercoat 106 are optional configurations, so it is not necessary to form one or both of them.
- the first buffer layer 110 is then formed on the substrate 102 (FIG. 3B).
- the first buffer layer 110 can be formed by a sputtering method.
- the first buffer layer 110 contains aluminum oxide, for example, aluminum or aluminum oxide may be used as a target, and oxygen radicals may be irradiated during reactive sputtering with a mixed gas of argon and oxygen to form the first buffer layer 110.
- an aluminum oxide target may be sputtered with argon, and the resulting first buffer layer 110 may be subjected to oxygen radical treatment.
- the substrate 102 may be irradiated with oxygen plasma to form an oxygen-excessive layer on the surface of the substrate 102, an aluminum target may be sputtered thereon to form a thin aluminum film, and then the thin aluminum film may be converted into an aluminum oxide film by heating (annealing), thereby forming the first buffer layer 110.
- an aluminum target may be sputtered using argon or a mixed gas of argon and oxygen to form an aluminum thin film or an aluminum thin film containing aluminum oxide on the substrate 102, and then the aluminum may be oxidized by oxygen plasma or oxygen radical treatment to form the first buffer layer 110.
- the first buffer layer 110 may be formed by reactive sputtering using a mixed gas of argon, oxygen, and nitrogen, using, for example, an aluminum target or an aluminum oxide target. At this time, the obtained first buffer layer 110 may be subjected to oxygen radical treatment and/or nitrogen radical treatment. Alternatively, the first buffer layer 110 may be formed by reactive sputtering using a mixed gas of argon and nitrogen, using an aluminum oxide target. Alternatively, the first buffer layer 110 may be formed by sputtering an aluminum oxynitride target using argon.
- the substrate 102 may be irradiated with nitrogen dioxide plasma to oxynitride the surface of the substrate 102, followed by sputtering an aluminum target to form an aluminum thin film, and further annealing to oxynitride the aluminum, thereby forming the first buffer layer 110.
- an aluminum target may be sputtered with argon to form an aluminum thin film, and the aluminum thin film may be oxynitrided using oxygen and nitrogen plasma.
- the first buffer layer 110 may be formed by sputtering an aluminum target, an aluminum oxynitride target, or an aluminum oxide target with argon while simultaneously performing oxygen radical treatment and nitrogen radical irradiation.
- the first buffer layer 110 can be configured so that the oxygen concentration decreases as the distance from the substrate 102 increases. This allows aluminum oxide closer to a stoichiometric ratio to be formed on the upper surface of the first buffer layer 110.
- the oxygen partial pressure can be reduced as the film grows.
- annealing may be performed to promote crystallization and increase the density of the layer.
- the temperature at this time may be appropriately selected from the range of 500°C to 700°C, for example.
- the second buffer layer 112 is formed on the first buffer layer 110 (FIG. 3B).
- the second buffer layer 112 may also be formed by a sputtering method.
- the second buffer layer 112 may be formed by sputtering an aluminum nitride target with argon.
- the second buffer layer 112 may be formed by performing reactive sputtering on an aluminum target or an aluminum nitride target using a mixed gas of argon and nitrogen.
- the obtained second buffer layer 112 may be further subjected to nitrogen radical treatment.
- the second buffer layer 112 may be formed by sputtering an aluminum target or an aluminum nitride target with argon and irradiating the target with nitrogen radicals at the same time.
- the nitrogen concentration may also vary in the film thickness direction in the second buffer layer 112.
- the nitrogen concentration may be controlled by controlling the partial pressure of nitrogen in reactive sputtering, or the nitrogen concentration on the surface of the second buffer layer 112 may be increased by nitrogen radical treatment.
- the second buffer layer 112 may be annealed to promote crystallization and increase the density of the layer.
- the temperature at this time may be appropriately selected from the range of 500°C to 700°C, for example.
- first buffer layer 110 and the second buffer layer 112 are formed successively in the same chamber, or in separate chambers while maintaining a vacuum state without returning to atmospheric conditions. This makes it possible to prevent impurities from being mixed into the interface between the first buffer layer 110 and the second buffer layer 112, and to more effectively promote crystallization of the second buffer layer 112.
- a gallium nitride layer 120 is formed on the second buffer layer 112, and semiconductor layers, that is, an n-type cladding layer 122, a light-emitting layer 124, and a p-type cladding layer 126 are sequentially formed thereon (FIG. 3C).
- semiconductor layers that is, an n-type cladding layer 122, a light-emitting layer 124, and a p-type cladding layer 126 are sequentially formed thereon (FIG. 3C).
- These layers can also be formed by using a sputtering method.
- these layers can be formed by sputtering a semiconductor target such as gallium nitride with argon in the presence of plasma.
- a target containing the dopant can be used.
- a gallium nitride target and a target for the dopant can be sputtered simultaneously.
- a light-emitting layer 124 in which an indium gallium nitride film and a gallium nitride film are alternately stacked can be formed.
- the light-emitting layer 124 is an indium gallium nitride film
- a gallium nitride target and an indium target are sputtered simultaneously
- a gallium nitride film is formed, a gallium nitride target is sputtered, thereby forming the light-emitting layer 124 in which an indium gallium nitride film and a gallium nitride film are alternately stacked.
- the n-type cladding layer 122 to the p-type cladding layer 126 are patterned.
- the patterning is performed so that a plurality of stacked bodies including the n-type cladding layer 122, the light-emitting layer 124, and the p-type cladding layer 126 are arranged in an island shape on the gallium nitride layer 120. Since each stacked body constitutes one light-emitting device 100, this method makes it possible to form a plurality of light-emitting devices 100 that share the gallium nitride layer 120 on one substrate 102.
- the patterning can be performed by applying known photolithography, so a detailed description will be omitted.
- the anode 128 and the cathode 130 are formed on the p-type cladding layer 126 and the n-type cladding layer 122, respectively (FIG. 4B).
- the anode 128 and the cathode 130 may be formed by using a method such as vacuum deposition, electron beam deposition, CVD, or sputtering.
- a method such as vacuum deposition, electron beam deposition, CVD, or sputtering.
- one or more films containing a silicon-containing inorganic compound are formed to cover the anode 128 and the cathode 130 using a CVD or sputtering method, and then the protective film 140 is etched to expose parts of the anode 128 and the cathode 130.
- the protective film 140 is also formed on the side surfaces of the substrate 102 (FIG. 4C).
- the substrate 102 is cut along the dotted lines in FIG. 4C to obtain the light-emitting element 100 shown in FIG. 1A.
- the first buffer layer 110 through the p-type cladding layer 126 can all be formed by sputtering. Therefore, the temperature during film formation is from room temperature to less than 600°C, typically 100°C or higher and 400°C or lower. Therefore, multiple light-emitting elements 100 can be manufactured using a substrate 102 containing inexpensive amorphous glass.
- the gallium nitride layer 120 to the p-type cladding layer 126 are formed on the second buffer layer 112. Therefore, even without applying the vapor phase epitaxial growth that has been conventionally used to form inorganic semiconductor layers, the semiconductor particles expelled by sputtering the semiconductor target are deposited to form each layer, and are simultaneously induced by the second buffer layer 112 to be effectively c-axis oriented. As a result, high temperatures are not required when forming the p-type cladding layer 126 from the first buffer layer 110, and each layer can have high crystallinity, and the light emitting device 100 can exhibit excellent characteristics as an LED.
- FIG. 5A a schematic end view of a high electron mobility field-effect transistor 150 is shown in FIG. 5A.
- the transistor 150 has a substrate 102, and includes a first buffer layer 110 and a second buffer layer 112 on the substrate 102, and an active layer (also called an electron transit layer) 152 on the second buffer layer 112.
- the active layer 152 corresponds to the gallium nitride layer 120 of the light-emitting element 100 described in the first embodiment.
- the transistor 150 further includes an electron supply layer 158 on the active layer 152, and a pair of terminals (a first terminal 154 and a second terminal 156) located on the active layer 152 and electrically connected to the active layer 152 and the electron supply layer 158.
- the first terminal 154 and the second terminal 156 may be in contact with the active layer 152, or may be connected to the active layer 152 via the electron supply layer 158 (not shown).
- the transistor 150 further includes a gate electrode 162 that is in direct contact with the electron supply layer 158 or is provided on the electron supply layer 158 via a gate insulating film 160 of any configuration.
- the active layer 152 and the electron supply layer 158 are stacked to form a source/drain current path when the transistor 150 is driven.
- the active layer 152 and the electron supply layer 158 contain a group 13 element and a group 15 element.
- the active layer 152 and the electron supply layer 158 may contain undoped gallium nitride and n-type aluminum gallium nitride, respectively.
- the active layer 152 and the electron supply layer 158 may contain undoped gallium arsenide (GaAs) and n-type aluminum gallium arsenide (AlGaAs), respectively.
- the active layer 152 is provided on the second buffer layer 112 by using a sputtering method so as to be in contact with the second buffer layer 112. For this reason, high temperature film formation is not required as is required for epitaxial growth using MOCVD, and the active layer 152 and the electron supply layer 158 can be formed even when a substrate 102 containing amorphous glass is used. In addition, the crystallization in the c-axis direction of the active layer 152 and the electron supply layer 158 is promoted by the second buffer layer 112 acting as the base thereof.
- the second buffer layer 112 is not provided directly on the substrate 102 having a large lattice mismatch, but is provided on the first buffer layer 110 for alleviating the lattice mismatch, and therefore has a high c-axis orientation. Therefore, since the second buffer layer 112 also has a high c-axis orientation, it is possible to achieve a high c-axis orientation in these layers even if the active layer 152 and the electron supply layer 158 are formed by using a sputtering method. As a result, a transistor having a high electric field mobility can be provided.
- the first terminal 154, the second terminal 156, and the gate electrode 162 contain metals such as aluminum, gold, silver, tantalum, molybdenum, titanium, and copper, or alloys containing one or more of the above metals.
- the gate insulating film 160 which is an arbitrary configuration, contains, for example, silicon-containing inorganic compounds such as silicon oxide and silicon nitride, or so-called high-k materials such as hafnium silicate, zirconium silicate, hafnium oxide, and zirconium oxide. There are no restrictions on the method of forming these configurations, and vacuum deposition, electron beam deposition, CVD, and sputtering can be appropriately adopted. Among them, the first terminal 154, the second terminal 156, the gate insulating film 160, and the gate electrode 162 can be efficiently formed by using the sputtering method and the electron beam deposition method, which have a high film formation rate.
- the transistor according to this embodiment may be a so-called metal insulator film field effect transistor (MISFET).
- MISFET metal insulator film field effect transistor
- the active layer 152 may be formed by a stack of a first active layer 152-1 including a p-type gallium nitride layer and a second active layer 152-2 located on the first active layer 152-1 and including an i-type or n-type gallium nitride layer, without providing the electron supply layer 158.
- the second active layer 152-2 may be provided in a divided manner between the first active layer 152-1 and the first terminal 154, and between the first active layer 152-1 and the second terminal 156, so as to form a source region and a drain region on the first active layer 152-1, respectively.
- the active layer 152 which determines its characteristics, is provided on the second buffer layer 112, which is provided on the first buffer layer 110 that alleviates the lattice constant mismatch between the substrate 102 and the second buffer layer 112. Therefore, the c-axis orientation of the active layer 152 is promoted on the second buffer layer 112, whose c-axis orientation has been improved by the first buffer layer 110, and as a result, the active layer 152 has high crystallinity. This allows the transistor 170 to have high electric field mobility.
- a display device may be combined as appropriate by a person skilled in the art to add or remove components or modify the design, or to add or omit processes or modify conditions, and this is also within the scope of the present invention, provided that the gist of the present invention is maintained.
- 100 light emitting element, 102: substrate, 104: overcoat, 106: undercoat, 110: first buffer layer, 112: second buffer layer, 114: third buffer layer, 116: fourth buffer layer, 120: gallium nitride layer, 122: n-type cladding layer, 124: light emitting layer, 126: p-type cladding layer, 128: anode, 130: cathode, 140: protective film, 150: transistor, 152: active layer, 152-1: first active layer, 152-2: second active layer, 154: first terminal, 156: second terminal, 158: electron supply layer, 160: gate insulating film, 162: gate electrode, 170: transistor
Landscapes
- Led Devices (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202380067836.0A CN119949053A (zh) | 2022-10-05 | 2023-08-08 | 发光元件及发光元件的制造方法 |
| JP2024555637A JP7807567B2 (ja) | 2022-10-05 | 2023-08-08 | 発光素子および発光素子の製造方法 |
| US19/053,507 US20250194303A1 (en) | 2022-10-05 | 2025-02-14 | Light-emitting element and manufacturing method of the light-emitting element |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022160638 | 2022-10-05 | ||
| JP2022-160638 | 2022-10-05 |
Related Child Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| US19/053,507 Continuation US20250194303A1 (en) | 2022-10-05 | 2025-02-14 | Light-emitting element and manufacturing method of the light-emitting element |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2024075388A1 true WO2024075388A1 (ja) | 2024-04-11 |
Family
ID=90607922
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/028862 Ceased WO2024075388A1 (ja) | 2022-10-05 | 2023-08-08 | 発光素子および発光素子の製造方法 |
Country Status (4)
| Country | Link |
|---|---|
| US (1) | US20250194303A1 (cg-RX-API-DMAC7.html) |
| JP (1) | JP7807567B2 (cg-RX-API-DMAC7.html) |
| CN (1) | CN119949053A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2024075388A1 (cg-RX-API-DMAC7.html) |
Cited By (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025239101A1 (ja) * | 2024-05-15 | 2025-11-20 | 株式会社ジャパンディスプレイ | 積層構造体、発光素子、および半導体装置 |
| WO2026018570A1 (ja) * | 2024-07-19 | 2026-01-22 | 株式会社ジャパンディスプレイ | 積層構造体 |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2009231745A (ja) * | 2008-03-25 | 2009-10-08 | Showa Denko Kk | Iii族窒化物半導体発光素子、iii族窒化物半導体発光素子の製造方法、及びランプ |
| JP2011091402A (ja) * | 2009-10-21 | 2011-05-06 | Lg Innotek Co Ltd | 発光素子、発光素子の製造方法 |
| JP2017152655A (ja) * | 2016-02-26 | 2017-08-31 | 株式会社豊田中央研究所 | 半導体装置 |
| JP2021530856A (ja) * | 2018-07-09 | 2021-11-11 | ソウル バイオシス カンパニー リミテッドSeoul Viosys Co., Ltd. | 発光装置及びその製造方法 |
Family Cites Families (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5741724A (en) * | 1996-12-27 | 1998-04-21 | Motorola | Method of growing gallium nitride on a spinel substrate |
-
2023
- 2023-08-08 CN CN202380067836.0A patent/CN119949053A/zh active Pending
- 2023-08-08 JP JP2024555637A patent/JP7807567B2/ja active Active
- 2023-08-08 WO PCT/JP2023/028862 patent/WO2024075388A1/ja not_active Ceased
-
2025
- 2025-02-14 US US19/053,507 patent/US20250194303A1/en active Pending
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2009231745A (ja) * | 2008-03-25 | 2009-10-08 | Showa Denko Kk | Iii族窒化物半導体発光素子、iii族窒化物半導体発光素子の製造方法、及びランプ |
| JP2011091402A (ja) * | 2009-10-21 | 2011-05-06 | Lg Innotek Co Ltd | 発光素子、発光素子の製造方法 |
| JP2017152655A (ja) * | 2016-02-26 | 2017-08-31 | 株式会社豊田中央研究所 | 半導体装置 |
| JP2021530856A (ja) * | 2018-07-09 | 2021-11-11 | ソウル バイオシス カンパニー リミテッドSeoul Viosys Co., Ltd. | 発光装置及びその製造方法 |
Cited By (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025239101A1 (ja) * | 2024-05-15 | 2025-11-20 | 株式会社ジャパンディスプレイ | 積層構造体、発光素子、および半導体装置 |
| WO2026018570A1 (ja) * | 2024-07-19 | 2026-01-22 | 株式会社ジャパンディスプレイ | 積層構造体 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7807567B2 (ja) | 2026-01-27 |
| JPWO2024075388A1 (cg-RX-API-DMAC7.html) | 2024-04-11 |
| US20250194303A1 (en) | 2025-06-12 |
| CN119949053A (zh) | 2025-05-06 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US20250194303A1 (en) | Light-emitting element and manufacturing method of the light-emitting element | |
| CN110112269B (zh) | 发光二极管外延片及其制备方法 | |
| WO2010100844A1 (ja) | 窒化物半導体素子及びその製造方法 | |
| CN102017082A (zh) | Ⅲ族氮化物半导体元件及其制造方法、ⅲ族氮化物半导体发光元件及其制造方法和灯 | |
| JP6165602B2 (ja) | n型負電極の形成方法、およびIII族窒化物半導体発光素子 | |
| TWI580074B (zh) | Semiconductor light emitting element | |
| JP2008047864A (ja) | 窒化物系半導体発光素子の製造方法 | |
| WO2011055664A1 (ja) | 半導体発光素子および半導体発光素子の製造方法 | |
| CN103503148A (zh) | 半导体层叠体及其制造方法以及半导体元件 | |
| JP7146589B2 (ja) | 半導体発光素子および半導体発光素子の製造方法 | |
| US20090045393A1 (en) | Nitride semiconductor device and method for manufacturing the same | |
| US20250380541A1 (en) | Semiconductor device and manufacturing method thereof | |
| JP2003060212A (ja) | シヨットキバリアダイオード及びその製造方法 | |
| WO2016002419A1 (ja) | 窒化物半導体発光素子 | |
| KR20070072826A (ko) | 질화갈륨계 발광다이오드 소자 및 그의 제조방법 | |
| JP7785929B2 (ja) | 半導体デバイス及びその作製方法 | |
| CN109411581B (zh) | 一种发光二极管外延片及其制造方法 | |
| CN109273571A (zh) | 一种氮化镓基发光二极管外延片及其制作方法 | |
| JP3665243B2 (ja) | 窒化物半導体素子及びその製造方法 | |
| CN101276864A (zh) | 发光元件 | |
| CN109473511B (zh) | 一种氮化镓基发光二极管外延片及其生长方法 | |
| WO2024116849A1 (ja) | 整流素子 | |
| JP2008130891A (ja) | Iii族窒化物化合物半導体発光素子の製造方法、及びiii族窒化物化合物半導体発光素子、並びにランプ | |
| JPH10303510A (ja) | Iii 族窒化物半導体素子およびその製造方法 | |
| JPH10341036A (ja) | 半導体基板、半導体素子及びそれらの製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23874521 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2024555637 Country of ref document: JP |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202380067836.0 Country of ref document: CN |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| WWP | Wipo information: published in national office |
Ref document number: 202380067836.0 Country of ref document: CN |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 23874521 Country of ref document: EP Kind code of ref document: A1 |