WO2023243711A1 - 熱伝導性組成物及び熱伝導性部材 - Google Patents

熱伝導性組成物及び熱伝導性部材 Download PDF

Info

Publication number
WO2023243711A1
WO2023243711A1 PCT/JP2023/022400 JP2023022400W WO2023243711A1 WO 2023243711 A1 WO2023243711 A1 WO 2023243711A1 JP 2023022400 W JP2023022400 W JP 2023022400W WO 2023243711 A1 WO2023243711 A1 WO 2023243711A1
Authority
WO
WIPO (PCT)
Prior art keywords
component
thermally conductive
conductive composition
group
content
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/022400
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
裕美 須田
達矢 岩本
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Sekisui Polymatech Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Sekisui Polymatech Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd, Sekisui Polymatech Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to EP23824001.4A priority Critical patent/EP4541866A4/en
Priority to CN202380046100.5A priority patent/CN119343425A/zh
Priority to US18/874,341 priority patent/US20250376591A1/en
Priority to KR1020247040925A priority patent/KR20250024921A/ko
Priority to JP2023562694A priority patent/JP7455343B1/ja
Publication of WO2023243711A1 publication Critical patent/WO2023243711A1/ja
Priority to JP2024033259A priority patent/JP2024061766A/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L83/00—Compositions of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon only; Compositions of derivatives of such polymers
    • C08L83/04—Polysiloxanes
    • C08L83/06—Polysiloxanes containing silicon bound to oxygen-containing groups
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09K—MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
    • C09K5/00—Heat-transfer, heat-exchange or heat-storage materials, e.g. refrigerants; Materials for the production of heat or cold by chemical reactions other than by combustion
    • C09K5/08—Materials not undergoing a change of physical state when used
    • C09K5/14—Solid materials, e.g. powdery or granular
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/06—Preparatory processes
    • C08G77/08—Preparatory processes characterised by the catalysts used
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/14—Polysiloxanes containing silicon bound to oxygen-containing groups
    • C08G77/18—Polysiloxanes containing silicon bound to oxygen-containing groups to alkoxy or aryloxy groups
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/01—Use of inorganic substances as compounding ingredients characterized by their specific function
    • C08K3/013—Fillers, pigments or reinforcing additives
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/18—Oxygen-containing compounds, e.g. metal carbonyls
    • C08K3/20—Oxides; Hydroxides
    • C08K3/22—Oxides; Hydroxides of metals
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L83/00—Compositions of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon only; Compositions of derivatives of such polymers
    • C08L83/04—Polysiloxanes
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W40/00—Arrangements for thermal protection or thermal control
    • H10W40/20—Arrangements for cooling
    • H10W40/25—Arrangements for cooling characterised by their materials
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/12—Polysiloxanes containing silicon bound to hydrogen
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/20—Polysiloxanes containing silicon bound to unsaturated aliphatic groups
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/18—Oxygen-containing compounds, e.g. metal carbonyls
    • C08K3/20—Oxides; Hydroxides
    • C08K3/22—Oxides; Hydroxides of metals
    • C08K2003/2227—Oxides; Hydroxides of metals of aluminium
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/001—Conductive additives
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L2205/00—Polymer mixtures characterised by other features
    • C08L2205/02—Polymer mixtures characterised by other features containing two or more polymers of the same C08L -group
    • C08L2205/025—Polymer mixtures characterised by other features containing two or more polymers of the same C08L -group containing two or more polymers of the same hierarchy C08L, and differing only in parameters such as density, comonomer content, molecular weight, structure
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L2314/00—Polymer mixtures characterised by way of preparation
    • C08L2314/08—Polymer mixtures characterised by way of preparation prepared by late transition metal, i.e. Ni, Pd, Pt, Co, Rh, Ir, Fe, Ru or Os, single site catalyst

Definitions

  • the present invention relates to a thermally conductive composition and a thermally conductive member.
  • Curable and liquid thermally conductive compositions are widely known. For example, they are filled between a heating element and a heat radiating element, and then hardened to form a cured product, which absorbs the heat generated by the heating element. It is used as a heat conductive member such as a heat dissipation gap filler that transmits heat to a heat dissipation body.
  • a heat conductive member such as a heat dissipation gap filler that transmits heat to a heat dissipation body.
  • silicone thermally conductive compositions containing an organopolysiloxane and a thermally conductive filler have been widely used as thermally conductive compositions.
  • Patent Document 1 describes (A) organopolysiloxane having two alkenyl groups in one molecule, (B) organohydrogenpolysiloxane having two Si-H groups in one molecule, (C ) organohydrogenpolysiloxane having three or more Si-H groups in one molecule, (D) at least one compound selected from the following (D1) and (D2), (D1) one alkenyl in one molecule (D2) an organohydrogenpolysiloxane having one Si--H group in one molecule, (E) a platinum catalyst, and (F) a thermally conductive filler in the above (A) to ( E) A thermally conductive silicone gel composition is disclosed, which is characterized by curing a component containing 100 to 600% by volume when the total amount is 100% by volume.
  • Patent Document 1 describes that component (D) is used to adjust the molecular weight so that it does not become large, and it is possible to provide a thermally conductive silicone gel composition that is a gel-like cured product but has low oil bleed. It is shown. However, in Patent Document 1, it is assumed that the surface temperature of a heat-generating electronic component such as an IC package is about 80° C., and there is no mention of reliability at higher temperatures.
  • heat dissipation gap fillers formed from conventional thermally conductive silicone thermally conductive compositions are used for long periods of time in high-temperature environments of 150°C or higher, their hardness increases, making them difficult to use for heating elements and heat dissipation elements. Since peeling occurs, it is difficult to suppress an increase in thermal resistance.
  • the present invention has been made in view of the above problems, and provides a thermally conductive composition capable of obtaining a thermally conductive member in which increase in hardness is suppressed even in a high-temperature environment of 150° C. or higher. That is the issue.
  • the present inventors have found that the addition reaction rate of silicone compounds having methacryloyl groups is slower than that of silicone compounds having alkenyl groups, which are the main ingredients, and has solved the above-mentioned problems. We found that it is possible to solve the problem. That is, the present invention provides the following [1] to [19].
  • thermally conductive composition according to any one of [1] to [8], which has a viscosity of 10 to 1000 Pa ⁇ s at a temperature of 25° C. and a shear rate of 3.16 (1/s).
  • thermally conductive composition according to any one of [1] to [9], wherein the thermally conductive filler contains aluminum oxide.
  • the first agent has a weight average molecular weight Mwa smaller than that of the first agent.
  • the electrical component according to [14] wherein the heating element is disposed at least either within the engine room or near the motor.
  • the electrical component according to [14] or [15] which is exposed to an environment of 150° C. or higher.
  • [17] A method of using a thermally conductive member obtained by curing the thermally conductive composition according to any one of [1] to [10], which is interposed between a heating element and a heat radiating element. [18] The method of use according to [17], wherein the heating element is a semiconductor element. [19] The method of use according to [17] or [18], wherein the heating element generates heat at 150°C or higher.
  • thermoly conductive composition capable of obtaining a thermally conductive member in which increase in hardness is suppressed even in a high temperature environment of 150° C. or higher.
  • the thermally conductive composition of the present invention has the following components (A) to (E). Components (A) to (E) will be explained in detail below.
  • Component (A) is an organopolysiloxane having an alkenyl group.
  • the thermally conductive composition can undergo an addition reaction with the organohydrogenpolysiloxane described below to form a cured product having appropriate hardness.
  • Component (A) can also be a mixture of a plurality of organopolysiloxanes having alkenyl groups.
  • the organopolysiloxane having an alkenyl group used as component (A) may be linear or branched, or may be a mixture of linear and branched, but it must be linear. is preferred.
  • the alkenyl group in component (A) may be contained either at the end or in the middle of the molecular chain of the polysiloxane structure of component (A), and may be contained at both the end and in the middle, but it should be contained at least at the end. It is preferable to contain it at both ends of the molecular chain formed by the polysiloxane structure, and even more preferably to contain it only at both ends.
  • the alkenyl group is not particularly limited, but includes, for example, those having 2 to 8 carbon atoms, including vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, etc.
  • the alkenyl group is preferably an alkenyl group directly bonded to a silicon atom.
  • the number of alkenyl groups in one molecule in component (A) may be 1 or more, preferably 2 or more, more preferably 2 to 4, still more preferably 2 to 3, even more preferably There are 2 pieces.
  • Component (A) may contain a plurality of components having different numbers of alkenyl groups in organopolysiloxane having alkenyl groups, but from the viewpoint of imparting a certain degree of curability to the thermally conductive composition, the main component is
  • the organopolysiloxane contained as a component preferably has two or more alkenyl groups, more preferably 2 to 4, still more preferably 2 to 3, even more preferably 2.
  • the main component means the component with the highest content rate among the organopolysiloxanes in component (A).
  • the organopolysiloxane having two or more alkenyl groups may account for, for example, 50 to 100% by mass, preferably 70 to 100% by mass of component (A).
  • the range indicated by "-" means a range from more than the predetermined numerical value written before and after "-" to less than the predetermined numerical value.
  • Remaining groups bonded to silicon atoms other than alkenyl groups include alkyl groups such as methyl, ethyl, propyl, butyl, hexyl, dodecyl, aryl groups such as phenyl, 2-phenylethyl, Specific examples include aralkyl groups such as 2-phenylpropyl group, and further specific examples include substituted hydrocarbon groups such as chloromethyl group and 3,3,3-trifluoropropyl group. Among these, methyl group is preferred from the viewpoint of ease of synthesis.
  • component (A) preferably does not have a hydrogen atom as a remaining group bonded to a silicon atom, that is, component (A) preferably does not contain a hydrosilyl group.
  • the organopolysiloxane of component (A) may be used alone or in combination of two or more.
  • the weight average molecular weight M wa of the component (A) may be larger than the weight average molecular weight M wd of the component (D), as described below, but the hardness of the cured product It is preferably 12,000 or more, and 15,000 or more, from the viewpoint of easily suppressing the increase in crosslinking density, preventing the crosslink density from becoming too high in the cured product, and making it easier to maintain flexibility after curing. More preferably, it is 18,000 or more.
  • M wa is preferably 35,000 or less, more preferably 32,000 or less, from the viewpoint of preventing the thermally conductive composition from becoming highly viscous or imparting a certain level of reactivity. , more preferably 27,000 or less.
  • component (A) at 25°C is not particularly limited, but is, for example, 80 to 5000 mPa ⁇ s, preferably 150 to 2500 mPa ⁇ s, more preferably 200 to 1500 mPa ⁇ s, and still more preferably 250 to 800 mPa ⁇ s. .
  • component (A) may be blended as a mixture with component (B), which will be described later. , preferably 150 to 2500 mPa ⁇ s, more preferably 200 to 1500 mPa ⁇ s, even more preferably 250 to 800 mPa ⁇ s.
  • the viscosity of component (A) or a mixture of components (A) and (B) By setting the viscosity of component (A) or a mixture of components (A) and (B) to the above lower limit value or higher, the crosslinking density of the cured product is prevented from becoming too high, and the flexibility after curing is improved. Easier to maintain. Moreover, by setting it below the said upper limit, a thermally conductive composition can be prevented from becoming highly viscous. Furthermore, by controlling the viscosity within the above range, it becomes easier to appropriately adjust the reactivity of component (A) or components (A) and (B).
  • component (A) is such that the viscosity at 25°C of component (A) blended in the first part is adjusted to the above viscosity range, and The viscosity of the blended mixture of component (A) and component (B) at 25° C. may be adjusted to the above viscosity range.
  • the content of component (A) is not particularly limited, but is, for example, 20 to 70% by mass, preferably 25 to 60% by mass, more preferably 30% by mass, based on the total amount of organopolysiloxane contained in the thermally conductive composition. ⁇ 50% by mass.
  • the organopolysiloxane contained in the total amount of organopolysiloxane is the sum of components (A), (B), and (D) that contribute to the addition reaction, as well as the component (F) that does not undergo the addition reaction.
  • Component (B) is an organohydrogenpolysiloxane having a hydrosilyl group.
  • the thermally conductive composition can undergo an addition reaction with the (A) component and the (D) component to form a cured product having appropriate hardness.
  • Component (B) may be linear or branched, or may be a mixture of linear and branched, but is preferably linear.
  • the hydrosilyl group may be contained either at the end of the molecular chain of the polysiloxane structure or in the middle of the molecular chain, and may be contained at both the end and the middle, but it should be contained at least at the end. It is more preferable, and it is more preferable to contain hydrosilyl groups at both ends of the molecular chain of the polysiloxane structure.
  • the number of hydrosilyl groups in one molecule in component (B) is not particularly limited and may be one or more, but preferably two or more, more preferably 2 to 25, and even more preferably 2 to 20. It is.
  • a component (B-1) having two hydrosilyl groups and a component (B-2) having three or more hydrosilyl groups may be used in combination.
  • the component having two hydrosilyl groups is not particularly limited, but it is preferable, for example, to be linear and to contain hydrosilyl groups at both ends of the molecular chain of the polysiloxane structure.
  • the number of hydrosilyl groups in one molecule is preferably 3 to 25, more preferably 3 to 20.
  • the remaining groups bonded to silicon atoms other than the hydrosilyl group include alkyl groups such as methyl group, ethyl group, propyl group, butyl group, hexyl group, and dodecyl group, aryl groups such as phenyl group, Examples include aralkyl groups such as 2-phenylethyl group and 2-phenylpropyl group, and further specific examples include substituted hydrocarbon groups such as chloromethyl group and 3,3,3-trifluoropropyl group. Among these, methyl group is preferred from the viewpoint of ease of synthesis.
  • component (B) preferably does not have an alkenyl group as the remaining group bonded to the silicon atom, that is, component (B) preferably does not contain an alkenyl group.
  • the organopolysiloxane of component (B) may be used alone or in combination of two or more.
  • the lower limit of the viscosity of component (B) at 25° C. is not particularly limited, but is, for example, 10 mPa ⁇ s or more, preferably 40 mPa ⁇ s or more, and more preferably 80 mPa ⁇ s or more.
  • the upper limit of the viscosity of component (B) at 25° C. is not particularly limited, but is, for example, 2000 mPa ⁇ s or less, preferably 1500 mPa ⁇ s or less, more preferably 1200 mPa ⁇ s or less. Further, the viscosity of component (B) at 25° C.
  • the viscosity of the component (B) is not particularly limited, but is, for example, 10 to 2000 mPa ⁇ s, preferably 40 to 1500 mPa ⁇ s, and more preferably 80 to 1200 mPa ⁇ s.
  • the content of component (B) may be appropriately selected so as to adjust the content ratio H/Vi, etc. described later, within a predetermined range, and is not particularly limited.
  • the amount is, for example, 3 to 35% by weight, preferably 5 to 30% by weight, and more preferably 8 to 25% by weight, based on the total amount of polysiloxane.
  • metal oxides include aluminum oxide typified by alumina, magnesium oxide, zinc oxide, and the like.
  • metal nitrides include aluminum nitride.
  • metal hydroxides include aluminum hydroxide.
  • carbon materials include spherical graphite and diamond.
  • oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide.
  • metal oxides, metal nitrides, and carbon materials are preferable as the thermally conductive filler from the viewpoint of improving thermal conductivity, and among these, metal oxides are more preferable.
  • aluminum oxide, magnesium oxide, aluminum nitride, and diamond are preferable, and aluminum oxide is more preferable.
  • thermally conductive fillers may be used alone or in combination of two or more.
  • aluminum oxide in combination with at least one of diamond, magnesium oxide, and aluminum nitride.
  • aluminum oxide and aluminum hydroxide are preferable to be used together.
  • the lower limit of the average particle size of the thermally conductive filler is not particularly limited, but from the viewpoint of increasing thermal conductivity, it is preferably 0.1 ⁇ m or more, more preferably 0.3 ⁇ m or more, and 0.5 ⁇ m or more. It is more preferable that The upper limit of the average particle size of the thermally conductive filler is not particularly limited, but from the viewpoint of improving the fluidity of the thermally conductive composition, it is preferably 200 ⁇ m or less, more preferably 100 ⁇ m or less, and 70 ⁇ m or less. It is even more preferable that there be.
  • the average particle size of the thermally conductive filler is not particularly limited, but in order to satisfy both the above viewpoints, it is preferably 0.1 to 200 ⁇ m, more preferably 0.3 to 100 ⁇ m, and More preferably, the thickness is .5 to 70 ⁇ m.
  • the thermally conductive filler may be a small-particle thermally conductive filler with an average particle size of 0.1 ⁇ m or more and 5 ⁇ m or less, and a large-particle thermally conductive filler with an average particle size of more than 5 ⁇ m and 200 ⁇ m or less. preferable.
  • the filling rate can be increased.
  • the average particle size means the particle size (D50) at a volume integration of 50% in the particle size distribution of the thermally conductive filler determined by a laser diffraction/scattering method.
  • the lower limit of the content of the thermally conductive filler in the thermally conductive composition is preferably 150 parts by mass or more, more preferably 500 parts by mass, based on 100 parts by mass of the organopolysiloxane contained in the thermally conductive composition.
  • the amount is more preferably 1,000 parts by mass or more, and even more preferably 1,500 parts by mass or more.
  • the upper limit of the content of the thermally conductive filler in the thermally conductive composition is preferably 4000 parts by mass or less, more preferably The amount is 3,500 parts by mass or less, more preferably 3,200 parts by mass or less, even more preferably 3,000 parts by mass or less.
  • the content of the thermally conductive filler in the thermally conductive composition is preferably 150 to 4000 parts by mass, more preferably 500 to 4000 parts by mass, based on 100 parts by mass of organopolysiloxane contained in the thermally conductive composition.
  • the amount is 3500 parts by weight, more preferably 1000 to 3200 parts by weight, even more preferably 1500 to 3000 parts by weight.
  • the lower limit of the volume-based content of the thermally conductive filler is preferably 50% by volume or more, more preferably 70% by volume or more, even more preferably The content is 75% by volume or more, more preferably 80% by volume or more.
  • the upper limit of the volume-based content of the thermally conductive filler is preferably 95% by volume or less, more preferably 93% by volume or less, even more preferably It is 92 volume % or less, more preferably 90 volume % or less.
  • the volume-based content of the thermally conductive filler is preferably 50 to 95% by volume, more preferably 70 to 93% by volume, and even more preferably It is 75 to 92% by volume, more preferably 80 to 90% by volume.
  • the thermally conductive filler By setting the content of the thermally conductive filler to the above upper limit or less, the thermally conductive filler can be appropriately dispersed. Moreover, it is also possible to prevent the viscosity of the thermally conductive composition from becoming higher than necessary. Furthermore, by setting the content of the thermally conductive filler in the range from the lower limit value to the upper limit value above, a certain level of thermal conductivity can be imparted to the thermally conductive composition and its cured product, and the thermally conductive filler It is possible to appropriately disperse the materials and prevent the viscosity of the thermally conductive composition from becoming higher than necessary.
  • Component (D) is a polysiloxane compound having a methacryloyl group.
  • the weight average molecular weight M wd of component (D) is smaller than the weight average molecular weight M wa of component (A).
  • the thermally conductive composition contains the component (D) whose weight average molecular weight M wd is smaller than the weight average molecular weight M wa of the component (A), the hardness increases even in a high temperature environment of 150° C. or higher. can be suppressed.
  • alkenyl groups have a faster addition reaction rate than methacryloyl groups, so that the hydrosilyl group in component (B) and the hydrosilyl group in component (A) reacts preferentially with alkenyl groups.
  • a crosslinked structure is formed by components (A) and (B) through an addition reaction, components (A) and (B) become difficult to diffuse or move within the composition, and as a result, they do not react.
  • the unreacted alkenyl group in component (A) and the hydrosilyl group in component (B) remain. Thereafter, in the latter half of the process, the methacryloyl group in component (D) is removed from the hydrosilyl group in component (B) that has not fully reacted with the alkenyl group in component (A) (hereinafter referred to as “unreacted hydrosilyl group”). (also called).
  • the thermally conductive composition of the present invention contains component (D), which has a lower weight average molecular weight than component (A), so that the curing process in which a crosslinked structure is being formed by component (A) and component (B) is achieved.
  • component (D) has a small weight average molecular weight and therefore easily diffuses or moves within the crosslinked structure, making it easier for the methacryloyl group of component (D) to react with unreacted hydrosilyl groups. Therefore, the remaining amount of unreacted hydrosilyl groups in the thermally conductive composition can be reduced, and after the composition has been cured, it is possible to suppress the increase in hardness of the cured product even if it is used in an environment of 150°C or higher. can. Further, the hardness of the cured product formed in the above curing process is substantially determined by the crosslinked structure formed by the reaction between the alkenyl group in component (A) and the hydrosilyl group in component (B). Ru.
  • M wa and M wd satisfy the following formula (1).
  • Mwd ⁇ 2.3 ⁇ Mwa ...(1)
  • the reactivity of component (D) with the unreacted hydrosilyl group can be increased, and in a high temperature environment of 150 ° C. or higher, Increase in hardness of the cured product of the thermally conductive composition can be suppressed.
  • M wa and M wd satisfy the following formula (1-A), and the formula (1-B ) is more preferably satisfied.
  • M wd ⁇ 2.5 ⁇ M wa ...(1-A) M wd ⁇ 3.0 ⁇ M wa ...(1-B)
  • t is preferably 30, and more preferably 10.
  • organopolysiloxane is used as the polysiloxane compound used as component (D).
  • the organopolysiloxane of component (D) may be linear or branched, or may be a mixture of linear and branched, but is preferably linear.
  • the methacryloyl group may be contained either at the end of the molecular chain of the polysiloxane structure or in the middle of the molecular chain, but it is preferably contained at the end, and more preferably at one end of the molecular chain of the polysiloxane structure.
  • Component (D) preferably has one or more methacryloyl groups in its molecule, and preferably has one methacryloyl group from the viewpoint of obtaining a cured product with excellent heat resistance.
  • the methacryloyl group may be a methacryloyl group directly bonded to a silicon atom, but any divalent group (for example, a divalent saturated aliphatic hydrocarbon group, a group represented by -XO-) (however, is a divalent saturated aliphatic hydrocarbon group, and the divalent saturated aliphatic hydrocarbon group has, for example, 1 to 18 carbon atoms, preferably 1 to 6 carbon atoms, more preferably 2 to 4 carbon atoms.
  • XO- may be bonded to a silicon atom via an oxygen atom (preferably an oxygen atom is bonded to a methacryloyl group)) or an oxygen atom.
  • the lower limit of M wd is not particularly limited, but from the viewpoint of reducing the viscosity of the thermally conductive composition, it is preferably 800 or more, more preferably 1500 or more, and even more preferably 3000 or more.
  • M wd is , preferably from 800 to 15,000, preferably from 1,500 to 12,000, and preferably from 3,000 to 7,000.
  • the content of component (D) may be appropriately selected so as to adjust the content ratio H/Vi, etc. described later, within a desired range, and is not particularly limited. For example, it is 1% by mass or more, preferably 2% by mass or more, more preferably 3% by mass or more, still more preferably 4% by mass or more, based on the total amount of siloxane. Further, for example, it is 55% by mass or less, preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 30% by mass or less.
  • component (D) is not particularly limited, but is, for example, 1 to 55% by mass, preferably 2 to 50% by mass, based on the total amount of organopolysiloxane contained in the thermally conductive composition. More preferably 3 to 45% by weight, still more preferably 4 to 30% by weight.
  • the thermally conductive composition of the present invention further contains, as component (F), an organopolysiloxane having no addition reactive group.
  • component (F) an organopolysiloxane having no addition reactive group.
  • the thermally conductive composition of the present invention prevents more than a certain amount of the component from being incorporated into the crosslinked structure of the cured product, making it easier to improve flexibility. Moreover, it becomes easier to reduce the viscosity of the thermally conductive composition, and it becomes easier to improve handleability.
  • the addition reaction group means a functional group that reacts by an addition reaction, and typical examples thereof include an alkenyl group, a methacryloyl group, an acryloyl group, a hydrosilyl group, and the like.
  • Component (F) includes (F-1) silicone oil and (F-2) organopolysiloxane having at least one alkoxy group.
  • Component (F) may contain either one of component (F-1) or component (F-2), but preferably contains at least component (F-2). By containing component (F-2), the viscosity of the thermally conductive composition can be further reduced. When the thermally conductive composition contains component (F-2), it may further contain component (F-1).
  • Component (F-2) may be linear or branched, or a mixture of linear and branched, but is preferably linear.
  • any organopolysiloxane having at least one alkoxy group may be used, but an organopolysiloxane having at least one alkoxy group at the molecular chain end of a polysiloxane structure is preferable, and one terminal More preferred are organopolysiloxanes that only have at least one alkoxy group.
  • Component has an alkoxy group, especially an alkoxy group at the end, so that it easily reacts or interacts with functional groups present on the surface of the thermally conductive filler, and has a polysiloxane structure. It is presumed that this combination reduces the friction of the filler and makes it easier to lower the viscosity of the thermally conductive composition.
  • Examples of the branched alkyl group include isopropyl group, tert-butyl group, isobutyl group, 2-methylundecyl group, and 1-hexylheptyl group.
  • Examples of the cyclic alkyl group include a cyclopentyl group, a cyclohexyl group, a cyclododecyl group, and the like.
  • Examples of the aryl group include phenyl group, tolyl group, xylyl group, and the like.
  • Examples of the aralkyl group include a benzyl group, a phenethyl group, and a 2-(2,4,6-trimethylphenyl)propyl group.
  • Examples of the halogenated alkyl group include 3,3,3-trifluoropropyl group and 3-chloropropyl group.
  • R 1 to R 5 , m, and n in formula (X) are preferably as follows from the viewpoint of enhancing the viscosity reduction effect.
  • R 1 in formula (X) is preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 2 to 6 carbon atoms, and particularly preferably a butyl group.
  • R 2 , R 4 , and R 5 in formula (X) are each independently preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably methyl. It is the basis.
  • R 3 in formula (X) is an oxygen atom or a divalent hydrocarbon group, and preferably a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a propylene group, a butylene group, a methylethylene group, and among them, an ethylene group is preferred.
  • the content of component (F) in the thermally conductive composition is, for example, 3% by mass or more and, for example, 63% by mass or less, based on the total amount of organopolysiloxane contained in the thermally conductive composition.
  • the lower limit of the content of component (F) in the thermally conductive composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more.
  • the upper limit of the content of component (F) in the thermally conductive composition is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.
  • the upper limit of the content of component (F) in the thermally conductive composition is preferably 3 to 63% by mass, more preferably 5 to 50% by mass, even more preferably 10 to 40% by mass, and even more preferably 15 to 63% by mass. 35% by mass is even more preferred.
  • component (F) preferably contains component (F-2).
  • the lower limit of the content of component (F-2) in the thermally conductive composition is preferably 2% by mass or more, and 4% by mass or more, based on the total amount of organopolysiloxane contained in the thermally conductive composition.
  • the content is more preferably 8% by mass or more.
  • the upper limit of the content of component (F-2) in the thermally conductive composition is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
  • the content of component (F-2) in the thermally conductive composition is preferably 2 to 40% by mass, more preferably 4 to 30% by mass, and even more preferably 8 to 20% by mass.
  • a thermally conductive composition containing component (F-2) at or above the above lower limit value has a viscosity of the thermally conductive composition by containing component (F-2) in a certain amount or more among components (F) This makes it easier to reduce
  • component (F) below the above upper limit, a certain level of curability can be imparted to the thermally conductive composition, making it easier to obtain a cured product with desired physical properties, and making it easier to prevent bleed-out after curing. .
  • the lower limit of the total content of components (A), (B), (D), and (F) is more preferably 3% by mass or more, even more preferably 3% by mass, based on the total amount of the thermally conductive composition.
  • the content is .5% by mass or more, more preferably 4% by mass or more.
  • the upper limit of the total content of components (A), (B), (D), and (F) is more preferably 20% by mass or less, and even more preferably 15% by mass based on the total amount of the thermally conductive composition.
  • the total content of components (A), (B), (D), and (F) is more preferably 3 to 20% by mass, and even more preferably 3.5% by mass based on the total amount of the thermally conductive composition. ⁇ 15% by weight, even more preferably 4 ⁇ 10% by weight.
  • additives can be contained in the thermally conductive composition of the present invention.
  • additives include reaction control agents, dispersants, flame retardants, plasticizers, antioxidants, and colorants.
  • each additive may be contained in either the first part or the second part, but it may be contained in both. The additive may be used by appropriately selecting one or more of these.
  • the total content of alkenyl groups and methacryloyl groups (hereinafter also referred to as "total Vi+Me content 1") in the total amount of organopolysiloxane contained in the thermally conductive composition is preferably 0.30 mmol/g or less.
  • the total Vi+Me content 1 is more preferably 0.25 mmol/g or less, still more preferably 0.15 mmol/g or less, even more preferably 0.12 mmol/g or less.
  • the total Vi + Me content 1 can be measured for each of the first part and the second part, but the preferable range of the above-mentioned total Vi + Me content 1 is for the first part and the second part. This is the combined value of the two drugs.
  • total Vi+Me content 2 The total content of alkenyl groups and methacryloyl groups (hereinafter also referred to as "total Vi+Me content 2") in the thermally conductive composition is preferably 8.0 ⁇ mol/g or less.
  • the total Vi+Me content 2 is more preferably 7.0 ⁇ mol/g or less, still more preferably 6.5 ⁇ mol/g or less, even more preferably 6.0 ⁇ mol/g or less.
  • the total Vi + Me content 2 is preferably 0.5 ⁇ mol/g or more, more preferably 1.0 ⁇ mol/g or more, and 2.0 ⁇ mol/g from the viewpoint of imparting constant curability and appropriate crosslinking density to the thermally conductive composition. /g or more is more preferable, and 3.0 ⁇ mol/g or more is even more preferable.
  • the total Vi + Me content 2 is preferably 0.5 to 8.0 ⁇ mol/g, and 1.0 to 1.0 ⁇ mol/g. 7.0 ⁇ mol/g is more preferable, 2.0 to 6.5 ⁇ mol/g is even more preferable, and even more preferably 3.0 to 6.0 ⁇ mol/g.
  • the content of the alkenyl group and the methacryloyl group described below can be a value calculated from the integral ratio of a 1H-NMR spectrum measured using an NMR measuring device.
  • Me content 1 is preferably 0.002 mmol/g or more from the viewpoint of sufficiently reducing the remaining amount of unreacted hydrosilyl groups in the thermally conductive composition and suppressing the increase in hardness in a high temperature environment after curing. It is more preferably 0.004 mmol/g or more, even more preferably 0.006 mmol/g or more, even more preferably 0.008 mmol/g or more.
  • the total Me content 2 is as follows: It is preferably 0.05 to 4.0 ⁇ mol/g, more preferably 0.1 to 3.5 ⁇ mol/g, even more preferably 0.2 to 3.0 ⁇ mol/g, and even more preferably 0.3 to 2.5 ⁇ mol/g. preferable.
  • the Me content is more preferably 0.15 or more, and even more preferably 0.19 or more, based on the total Vi+Me content.
  • the Me content is the total Vi + Me content. , it is more preferably 0.55 or less, and even more preferably 0.50 or less. Further, the Me content is more preferably 0.15 to 0.55, even more preferably 0.19 to 0.50 or more, based on the total Vi+Me content.
  • the content of alkenyl groups contained in component (A) (hereinafter referred to as "DVi content”) is preferably 0.17 or less, more preferably 0.15 or less, and 0. It is more preferably 10 or less, and even more preferably 0.05 or less.
  • the DVi content relative to the total Vi+Me content is preferably as low as possible, and may be 0 or more.
  • the thermally conductive composition of the present invention contains component (D), by satisfying the relationship of the above formula (4), the curability of the thermally conductive composition can be improved.
  • the thermally conductive composition Materials can be cured appropriately even at room temperature. Moreover, even in a high temperature environment of 150° C. or higher, the effect of suppressing the increase in hardness of the cured product of the thermally conductive composition is enhanced.
  • the above H/Vi is more preferably 0.95 or more, and even more preferably 1.05 or more.
  • the above H/Vi is more preferably 1.40 or less, and even more preferably 1.20 or less.
  • H/Vi is more preferably 0.95 to 1.40, and 1. 05 to 1.20 is more preferable.
  • the thermally conductive composition of the present invention can improve the curability of the thermally conductive composition, for example, can appropriately cure the thermally conductive composition even at room temperature. be able to. Moreover, even in a high temperature environment of 150° C. or higher, the effect of suppressing the increase in hardness of the cured product of the thermally conductive composition is enhanced.
  • H/(Vi+Me) is more preferably 0.50 or more, and even more preferably 0.55 or more.
  • H/(Vi+Me) is more preferably 1.05 or less, and even more preferably 0.95 or less.
  • H/(Vi+Me) is more preferably from 0.50 to 1.05, and even more preferably from 0.55 to 0.95.
  • the content ratio H/Vi and the content ratio H/(Vi+Me) can be calculated from the amount of functional groups of each component to be blended and the content of each component.
  • the amount of functional groups in each component to be blended can be calculated from the integral ratio of the 1H-NMR spectrum as described above.
  • formula (5-2) a methacryloyl group is contained in the thermally conductive composition, and the hardness of the cured product of the thermally conductive composition increases in a high temperature environment. Can be suppressed. H/(Vi+Me) ⁇ H/Vi...(5-2)
  • the lower limit of E2/E1 is not particularly limited, but is practically 1 or more, preferably 1.15 or more.
  • the type E hardness in the present invention is a value measured by a type E hardness meter according to JIS K 6253, which is the Japanese Industrial Standard.
  • the type E hardness (E2) of the thermally conductive composition satisfies the following formula (7-2). E2 ⁇ 80...(7-2)
  • the first part and the second part may be mixed and then left at 25° C. for 24 hours. The same applies to other hardness measurements.
  • the type E hardness (E2) is less than 80, it is easy to maintain the flexibility of the cured product in an environment of 150°C or higher, and it is easy to relieve stress such as vibration, so it will peel off from the heating element or heat radiating element. is less likely to occur. Therefore, when the cured product of the thermally conductive composition is used as a heat dissipation gap filler (thermally conductive member) in an environment of 150°C or higher, it is possible to prevent peeling from the heating element or heat dissipation element, and to prevent an increase in thermal resistance. Reliability can be maintained. From the viewpoint of flexibility and reliability, the type E hardness (E2) is preferably 75 or less, more preferably 73 or less, and even more preferably 70 or less.
  • the type E hardness (E2) is not particularly limited, but is, for example, 30 or more, preferably 40 or more, and more preferably 50 or more.
  • the Type E hardness (E2) is not particularly limited, but is, for example, 30 or more, preferably 40 or more, and more preferably 50 or more.
  • the hardness change expressed by the value of E3-E2 is the same as when heated at 150°C for a long period of time. Represents hardness change.
  • the lower the value of E3-E2 the less the change in performance even when used for a long period of time at a temperature of 150° C. or higher, which means that the long-term heat resistance is better.
  • the hardness change represented by the value of E3-E2 is preferably 6 or less, more preferably 4 or less, and preferably 2 or less. Note that the hardness change represented by the value of E3-E2 is not particularly limited, but is usually 0 or more.
  • the components (B-1) and (B-2) contained in component (B) satisfy the relationship of formula (1-2) below. Preferably, it is contained. b1/(b1+b2)>0.45...(1-2)
  • b1 is the concentration of hydrosilyl groups contained in component (B-1)
  • b2 is the concentration of hydrosilyl groups contained in component (B-2). Note that the concentration of hydrosilyl groups here refers to the concentration of hydrosilyl groups in the thermally conductive composition.
  • the organohydrogenpolysiloxane is not contained in the first part, but only in the second part. Therefore, in a two-part thermally conductive composition, it can also be said to mean the concentration of hydrosilyl groups in the second part. That is, component (B-1) and component (B-2) are preferably contained in the second agent so as to satisfy the relationship of formula (1-2).
  • the crosslinking points tend to become sparse, making it easier to maintain good flexibility of the cured product in an environment of 150° C. or higher. Therefore, when the cured product of the thermally conductive composition is used as a heat dissipation gap filler in an environment of 150°C or higher, peeling from the heating element or heat dissipation element is less likely to occur, and the problem of increased thermal resistance is less likely to occur. Improved reliability. Furthermore, due to the increased flexibility, for example, when made thick, it can exhibit cushioning properties and can be suitably used in environments where vibrations occur.
  • b1/(b1+b2) is preferably 0.48 or more, more preferably 0.50 or more, and even more preferably 0.52 or more. It is preferable that b1/(b1+b2) is less than 0.85. By setting b1/(b1+b2) to less than 0.85, it becomes easier to introduce a crosslinked structure into the cured product with an appropriate crosslinking density. Therefore, it becomes easier to maintain the hardness at a constant value even when heated at high temperatures for a long period of time, and it becomes easier to improve long-term heat resistance.
  • the thermally conductive composition is such that the Raman intensity p1 at 2160 cm -1 and the Raman intensity p2 at 2130 cm -1 in the Raman spectrum satisfy the following equation (1-1). preferable. p2/p1>3.00...(1-1)
  • the Raman intensity p1 at 2160 cm ⁇ 1 in the Raman spectrum is the Raman intensity at the peak wavelength derived from the hydrosilyl group contained in the middle of the molecular chain of the polysiloxane structure.
  • the Raman intensity p2 at 2130 cm ⁇ 1 in the Raman spectrum is the Raman intensity at the peak wavelength derived from the hydrosilyl group contained at the end of the molecular chain of the polysiloxane structure. Therefore, p2/p1 can be said to be an index indicating the amount of terminal hydrosilyl groups relative to the hydrosilyl groups contained in the middle of the molecular chain.
  • p2/p1 is preferably 3.10 or more, more preferably 3.20 or more, and even more preferably 3.30 or more. Further, p2/p1 is preferably less than 5.5.
  • the Raman intensity ratio H/(Vi+Me) is preferably 3.00 to 12.00, more preferably 4.00 to 10.00, and preferably 5.00 to 9.00. More preferred.
  • the Raman intensity ratio H/(Vi+Me) within the above range, the number of hydrosilyl groups and the total number of alkenyl groups and methacryloyl groups are balanced, and components (A), (B), and (D) are appropriately controlled. For example, curing can proceed appropriately even at room temperature. Further, it becomes easier to suppress increase in hardness in a high temperature environment after curing.
  • the Raman spectrum of the first agent and the Raman spectrum of the second agent first, the area C of the Si-O-Si peak appearing at a wave number of 490 cm -1 , the area D of the vinyl group peak appearing at a wave number of 1600 cm -1 , and , the area F of the peak of the hydrosilyl group appearing at a wave number of 2130 to 2160 cm ⁇ 1 is calculated. Next, the following calculations are performed using the area C as a reference, and the intensity error for each measurement is corrected and normalized.
  • an index of the ratio of hydrosilyl group/(vinyl group + methacryloyl group) is calculated using the following formula. Note that since there is a difference in Raman scattering intensity between a vinyl group and a methacryloyl group, the calculation is performed by multiplying by 0.5 as a correction coefficient.
  • the first part contains an organopolysiloxane having either an alkenyl group or a methacryloyl group (alkenyl group-containing organopolysiloxane), and (E) a hydrosilylation catalyst, Contains no organohydrogenpolysiloxane.
  • the second agent contains the organohydrogenpolysiloxane, but does not contain the (E) hydrosilylation catalyst.
  • at least one of the first agent and the second agent contains (C) a thermally conductive filler.
  • both the first part and the second part contain (C) a thermally conductive filler.
  • the thermally conductive filler may be contained in either the first part or the second part to form the thermally conductive composition, but as described above, the thermally conductive filler may be contained in either the first part or the second part. It is preferable that it is contained in both, and it is more preferable that it is contained approximately equally. Specifically, the ratio (mass ratio) of the content of the thermally conductive filler (E) in the second agent to the content of the thermally conductive filler (C) in the first agent is 0.67 to 1.
  • the viscosity VB of the binder resin in the thermally conductive composition can be measured in the same way, but in the case of a two-component type thermally conductive composition, the viscosity VB1, VB2 of the binder resin in the first part and the second part, respectively. It is also possible to roughly estimate the viscosity VB from
  • the viscosity V of the thermally conductive composition of the present invention under the conditions of a temperature of 25°C and a shear rate of 3.16 (1/s) is preferably 10 to 1000 Pa ⁇ s, and preferably 50 to 700 Pa ⁇ s. It is more preferable that it be 200 to 450 Pa ⁇ s. Since the thermally conductive composition has the above-mentioned viscosity, it has a predetermined fluidity before curing, and can be applied to narrow gaps and complicated shapes. When the thermally conductive composition is a two-part type, the viscosity V can be determined by mixing the first part and the second part and immediately measuring it. It is also possible to roughly estimate the viscosity value from the viscosities V1 and V2.
  • ) is preferably small from the viewpoint of making it easier to mix the thermally conductive composition uniformly.
  • ) between the first agent and the second agent may be, for example, 130 Pa ⁇ s or less, preferably 100 Pa ⁇ s or less, and 30 Pa ⁇ s or less. It is more preferable.
  • ) between the first agent and the second agent may be 0 Pa ⁇ s or more.
  • the viscosity V1 and V2 of the first agent and the second agent can be measured by the following method.
  • the shape of the thermally conductive member is not particularly limited, and may be sheet-like or may be used in other shapes.
  • the thickness of the thermally conductive member is not particularly limited, and can be used, for example, from 0.3 to 5 mm, preferably from 0.5 to 4 mm. In the present invention, since the thermally conductive member has flexibility, if its thickness is increased (for example, 0.5 mm or more), it can exhibit cushioning properties and can be suitably used in an environment where vibrations occur.
  • the first and second agents were filled into a 50cc two-liquid parallel cartridge (MIXPAC's 1:1 mixing cartridge "CDA050-01-PP"), and a static mixer (two-liquid mixing static mixer "MA6.3") was filled with the first and second agents.
  • -12S number of elements 6.3 mm x 12, discharge port inner diameter 1.5 mm
  • the thermally conductive composition (volume ratio 1:1, mass ratio 1:1) was mixed into a sample. Apply it to the release surface of a release-treated PET film ("SG2" manufactured by Panac Corporation) so that the thickness is 2 mm, and then apply another PET film (“SG2" manufactured by Panac Corporation) over the sample.
  • Sample 1A was obtained by leaving it for 24 hours at a temperature of 25° C. and a humidity of 50% RH. Five sheets of 30 mm square were punched out from the obtained sample 1A and stacked on top of each other, and the type E hardness was measured and the hardness was set as E1.
  • Sample 2A obtained in the same manner as above was placed inside a constant temperature bath set at 150° C. and left in the constant temperature bath for 250 hours. Sample 2A after being left for 250 hours was taken out from the constant temperature bath and cooled to 25° C., and the type E hardness of sample 2A was measured, giving a hardness of E2.
  • E2/E1 was also determined from the obtained hardnesses E1 and E2.
  • ⁇ Weight average molecular weight of component (A) and component (D)> The first and second agents containing component (A) and component (D) (hereinafter also referred to as "sample") were analyzed using a high performance liquid chromatograph (HPLC)-Raman microscope complex device (LC-Raman system: Shimadzu Corporation). The weight average molecular weight of each component was determined using a column manufactured by Shodex HK-404L (150 mm x 4.6 mm I.D., 3.5 ⁇ m). Specifically, each sample was dissolved in tetrahydrofuran to prepare a 0.2% by weight solution, and the solution was filtered through a 0.2 ⁇ m filter before being used for measurement.
  • HPLC high performance liquid chromatograph
  • the vinyl group was identified by a peak at 1600 cm -1 and the methacryloyl group was identified by a peak at 1640 cm -1 .
  • the weight average molecular weights of component (A) and component (D) contained in the thermally conductive composition were estimated based on the mixing ratio of the first agent and the second agent.
  • the first agent and the second agent were analyzed separately in the above, a mixture can be analyzed in the same way.
  • the weight average molecular weight of each component may be measured.
  • Organopolysiloxane 1 (component (A)): Organopolysiloxane having vinyl groups at both ends of the molecular chain (vinyl group content 0.17 mmol/g, viscosity 410 mPa ⁇ s, weight average molecular weight 25400)
  • Organopolysiloxane 4 (component (B)): Organopolysiloxane having hydrosilyl groups at both ends of the molecular chain (hydrosilyl group content 0.329 mmol/g, viscosity 128 mPa ⁇ s, weight average molecular weight 6000)
  • Organopolysiloxane 5 (component (D)): Organopolysiloxane having a methacryloyl group at one end of the molecular chain (methacryloyl group content 0.20 mmol/g, viscosity 65 mPa ⁇ s, weight average molecular weight 5000)
  • Organopolysiloxane 6 (component (D)): Organopolysiloxane having a methacryloyl group at one end of the molecular chain (methacryloyl group content 0.10 mmol/g, viscosity 177 mPa ⁇ s, weight average molecular weight 10,000)
  • Organopolysiloxane 7 An organopolysiloxane having a vinyl group at one end of the molecular chain (component (A), 50% by mass) and an organopolysiloxane having a vinyl group at both ends of the molecular chain (component (A), 25 % by mass) and a mixture of organopolysiloxane (component (F), 25% by mass) without vinyl groups (vinyl group content 0.22 mmol/g, viscosity 110 mPa ⁇ s, weight average molecular weight 5000)
  • Organopolysiloxane 8 ((F-1) component): Dimethyl silicone oil without hydrosilylation addition reaction group (viscosity 101 mPa ⁇ s)
  • Organopolysiloxane 9 ((F-2) component): Organopolysiloxane that does not have a hydrosilylation addition reaction group and has a trialkoxysilyl group at the end (viscosity 26 mPa ⁇ s)
  • Organopolysiloxane 10 (component (A)): Organopolysiloxane having vinyl groups at both ends of the molecular chain (vinyl group content 0.34 mmol/g, viscosity 110 mPa ⁇ s, weight average molecular weight 9200)
  • Organopolysiloxane 11 (component (A) and component (B)): An organopolysiloxane (component (A)) having vinyl groups at both ends of the molecular chain, and an organopolysiloxane (component (A)) having three or more hydrosilyl groups.
  • Examples 1 to 9 Comparative Examples 1 to 4
  • a first agent and a second agent were prepared according to the formulations shown in Tables 1 to 3 below.
  • Using a thermally conductive composition obtained by mixing the first agent and the second agent various physical properties were measured and various evaluations were performed.
  • the total Vi+Me content 1 is the total content of alkenyl groups and methacryloyl groups with respect to the total amount of organopolysiloxanes 1 to 9 in each of the first and second agents.
  • the total Vi+Me content 2 is the total content of alkenyl groups and methacryloyl groups with respect to the total amount of the thermally conductive composition (first part and second part).
  • the total Me content 1 is the total content of methacryloyl groups relative to the total amount of organopolysiloxanes 1 to 9 in each of the first and second agents.
  • the total Me content 2 is the total content of methacryloyl groups with respect to the total amount of the thermally conductive composition (first part and second part).
  • the amount of hydrosilyl groups 1 is the total content of hydrosilyl groups relative to the total amount of organopolysiloxanes 1 to 9 in each of the first and second agents.
  • the amount of hydrosilyl groups 2 is the total content of hydrosilyl groups with respect to the total amount of the thermally conductive composition (first part and second part).
  • the thermally conductive member formed from the thermally conductive composition that satisfies the requirements of the present invention was suppressed from increasing in hardness even when placed in a high temperature environment.
  • the thermally conductive members formed from the thermally conductive compositions of Comparative Examples 2 and 3 do not contain the component (D) and are unable to suppress the increase in hardness in a high-temperature environment. could not.
  • the thermally conductive composition of Comparative Example 1 could not be cured, it was not possible to form a thermally conductive member, and it was not possible to evaluate whether or not the increase in hardness was suppressed.
  • Comparative Example 4 in which the weight average molecular weight M wd of the component (D) was larger than the weight average molecular weight M wa of the component (A), the increase in hardness could not be suppressed in a high temperature environment.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Organic Chemistry (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Health & Medical Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Physics & Mathematics (AREA)
  • Combustion & Propulsion (AREA)
  • Thermal Sciences (AREA)
  • Materials Engineering (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Cooling Or The Like Of Electrical Apparatus (AREA)
PCT/JP2023/022400 2022-06-17 2023-06-16 熱伝導性組成物及び熱伝導性部材 Ceased WO2023243711A1 (ja)

Priority Applications (6)

Application Number Priority Date Filing Date Title
EP23824001.4A EP4541866A4 (en) 2022-06-17 2023-06-16 THERMOCONDUCTIVE COMPOSITION AND THERMOCONDUCTIVE ELEMENT
CN202380046100.5A CN119343425A (zh) 2022-06-17 2023-06-16 导热性组合物和导热性部件
US18/874,341 US20250376591A1 (en) 2022-06-17 2023-06-16 Heat-conductive composition and heat-conductive member
KR1020247040925A KR20250024921A (ko) 2022-06-17 2023-06-16 열전도성 조성물 및 열전도성 부재
JP2023562694A JP7455343B1 (ja) 2022-06-17 2023-06-16 熱伝導性組成物及び熱伝導性部材
JP2024033259A JP2024061766A (ja) 2022-06-17 2024-03-05 熱伝導性組成物及び熱伝導性部材

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP2022-098435 2022-06-17
JP2022098435 2022-06-17
JP2022138189 2022-08-31
JP2022-138189 2022-08-31

Publications (1)

Publication Number Publication Date
WO2023243711A1 true WO2023243711A1 (ja) 2023-12-21

Family

ID=89191462

Family Applications (2)

Application Number Title Priority Date Filing Date
PCT/JP2023/022400 Ceased WO2023243711A1 (ja) 2022-06-17 2023-06-16 熱伝導性組成物及び熱伝導性部材
PCT/JP2023/022402 Ceased WO2023243712A1 (ja) 2022-06-17 2023-06-16 熱伝導性組成物及び熱伝導性部材

Family Applications After (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/022402 Ceased WO2023243712A1 (ja) 2022-06-17 2023-06-16 熱伝導性組成物及び熱伝導性部材

Country Status (6)

Country Link
US (2) US20250304790A1 (cg-RX-API-DMAC7.html)
EP (2) EP4541867A4 (cg-RX-API-DMAC7.html)
JP (4) JP7414246B1 (cg-RX-API-DMAC7.html)
KR (2) KR20250024921A (cg-RX-API-DMAC7.html)
CN (2) CN119343425A (cg-RX-API-DMAC7.html)
WO (2) WO2023243711A1 (cg-RX-API-DMAC7.html)

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008160126A (ja) * 2007-12-21 2008-07-10 Shin Etsu Chem Co Ltd 電子部品の冷却構造
JP2009256428A (ja) * 2008-04-15 2009-11-05 Shin Etsu Chem Co Ltd 熱伝導性シリコーン組成物及び接着構造体並びに半導体装置
JP2016513151A (ja) * 2013-02-11 2016-05-12 ダウ コーニング コーポレーションDow Corning Corporation 官能基密集型ポリオルガノシロキサン及びシリコーン反応性希釈剤を含む硬化性シリコーン組成物
WO2019021826A1 (ja) * 2017-07-24 2019-01-31 東レ・ダウコーニング株式会社 多成分硬化型熱伝導性シリコーンゲル組成物、熱伝導性部材および放熱構造体
WO2020080256A1 (ja) * 2018-10-15 2020-04-23 デンカ株式会社 二液硬化型組成物セット、熱伝導性硬化物及び電子機器
WO2022075434A1 (ja) * 2020-10-09 2022-04-14 ダウ・東レ株式会社 熱伝導性シリコーン組成物および熱伝導性部材

Family Cites Families (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS6079792U (ja) 1983-11-09 1985-06-03 株式会社日立製作所 回路基板取付装置
JP4590253B2 (ja) * 2004-12-16 2010-12-01 東レ・ダウコーニング株式会社 オルガノポリシロキサンおよびシリコーン組成物
CN106414613B (zh) * 2014-04-09 2019-12-27 陶氏东丽株式会社 导热有机硅组合物和电气电子设备
JP6260519B2 (ja) * 2014-11-25 2018-01-17 信越化学工業株式会社 一液付加硬化型シリコーン組成物の保存方法及び硬化方法
EP3992252A4 (en) * 2019-06-26 2023-07-19 Sekisui Polymatech Co., Ltd. Thermally conductive composition package, and two-component curing type thermally conductive composition
CN110746926A (zh) * 2019-12-02 2020-02-04 扬州宏远新材料股份有限公司 一种具有自粘性的导热阻燃双组份电子灌封硅橡胶及其制备方法
CN113454165B (zh) 2020-01-06 2023-09-22 富士高分子工业株式会社 导热性硅胶组合物
FI4134392T3 (fi) * 2020-04-06 2025-09-24 Sekisui Chemical Co Ltd Hartsikoostumus, lämpöä säteilevä elementti ja elektroninen laite

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008160126A (ja) * 2007-12-21 2008-07-10 Shin Etsu Chem Co Ltd 電子部品の冷却構造
JP2009256428A (ja) * 2008-04-15 2009-11-05 Shin Etsu Chem Co Ltd 熱伝導性シリコーン組成物及び接着構造体並びに半導体装置
JP2016513151A (ja) * 2013-02-11 2016-05-12 ダウ コーニング コーポレーションDow Corning Corporation 官能基密集型ポリオルガノシロキサン及びシリコーン反応性希釈剤を含む硬化性シリコーン組成物
WO2019021826A1 (ja) * 2017-07-24 2019-01-31 東レ・ダウコーニング株式会社 多成分硬化型熱伝導性シリコーンゲル組成物、熱伝導性部材および放熱構造体
WO2020080256A1 (ja) * 2018-10-15 2020-04-23 デンカ株式会社 二液硬化型組成物セット、熱伝導性硬化物及び電子機器
WO2022075434A1 (ja) * 2020-10-09 2022-04-14 ダウ・東レ株式会社 熱伝導性シリコーン組成物および熱伝導性部材

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4541866A4 *

Also Published As

Publication number Publication date
JP2024061766A (ja) 2024-05-08
WO2023243712A1 (ja) 2023-12-21
KR20250024751A (ko) 2025-02-19
EP4541866A4 (en) 2026-06-24
JP2024039036A (ja) 2024-03-21
KR20250024921A (ko) 2025-02-20
US20250376591A1 (en) 2025-12-11
JPWO2023243712A1 (cg-RX-API-DMAC7.html) 2023-12-21
US20250304790A1 (en) 2025-10-02
JP7414246B1 (ja) 2024-01-16
EP4541866A1 (en) 2025-04-23
EP4541867A4 (en) 2026-06-24
JPWO2023243711A1 (cg-RX-API-DMAC7.html) 2023-12-21
EP4541867A1 (en) 2025-04-23
CN119343425A (zh) 2025-01-21
JP7455343B1 (ja) 2024-03-26
CN119256062A (zh) 2025-01-03

Similar Documents

Publication Publication Date Title
JP7134582B2 (ja) 熱伝導性ポリオルガノシロキサン組成物
KR102542191B1 (ko) 열전도성 폴리오르가노실록산 조성물
JP6194861B2 (ja) 熱伝導性シリコーン組成物及び熱伝導性シリコーン成型物
JP6075261B2 (ja) 熱伝導性シリコーン組成物及びその硬化物
KR101859617B1 (ko) 가열 경화형 열전도성 실리콘 그리스 조성물
JP5304623B2 (ja) 高熱伝導性ポッティング材の選定方法
KR102632046B1 (ko) 열전도성 폴리실록산 조성물의 제조 방법
KR20220121805A (ko) 열전도성 실리콘 조성물
KR20160058801A (ko) 실리콘조성물 및 열전도성 실리콘조성물의 제조방법
KR20210080376A (ko) 열전도성 실리콘 조성물 및 그의 경화물
EP4541858A1 (en) Silicone composition, heat dissipation member, and electronic device
JP7455343B1 (ja) 熱伝導性組成物及び熱伝導性部材
KR20210080351A (ko) 열전도성 실리콘 조성물 및 그의 경화물
JP2023184499A (ja) シリコーン組成物、放熱部材、及び電子機器
WO2023026615A1 (ja) 熱伝導性組成物
WO2024077435A1 (en) Thermally conductive silicone composition
JP2023184498A (ja) シリコーン組成物、放熱部材、及び電子機器
EP4379003A1 (en) Thermally conductive composition and cured product
KR20250172689A (ko) 폴리실록산 조성물
WO2023243706A1 (ja) シリコーン組成物、放熱部材、及び電子機器
JP2024164508A (ja) 熱伝導性シート

Legal Events

Date Code Title Description
ENP Entry into the national phase

Ref document number: 2023562694

Country of ref document: JP

Kind code of ref document: A

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23824001

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202380046100.5

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 18874341

Country of ref document: US

WWE Wipo information: entry into national phase

Ref document number: 2023824001

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 202380046100.5

Country of ref document: CN

ENP Entry into the national phase

Ref document number: 2023824001

Country of ref document: EP

Effective date: 20250117

WWP Wipo information: published in national office

Ref document number: 1020247040925

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 2023824001

Country of ref document: EP

WWP Wipo information: published in national office

Ref document number: 18874341

Country of ref document: US