WO2023181489A1 - 積層体及び積層体の製造方法 - Google Patents

積層体及び積層体の製造方法 Download PDF

Info

Publication number
WO2023181489A1
WO2023181489A1 PCT/JP2022/042287 JP2022042287W WO2023181489A1 WO 2023181489 A1 WO2023181489 A1 WO 2023181489A1 JP 2022042287 W JP2022042287 W JP 2022042287W WO 2023181489 A1 WO2023181489 A1 WO 2023181489A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
laminate
resin layer
inorganic
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/042287
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
佳彦 望月
諭史 長野
岳彦 原沢
友和 関
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fujifilm Corp
Original Assignee
Fujifilm Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fujifilm Corp filed Critical Fujifilm Corp
Priority to EP22933619.3A priority Critical patent/EP4501621A4/en
Priority to KR1020247030376A priority patent/KR20240151785A/ko
Priority to JP2024509737A priority patent/JPWO2023181489A1/ja
Priority to CN202280093717.8A priority patent/CN118900765A/zh
Publication of WO2023181489A1 publication Critical patent/WO2023181489A1/ja
Priority to US18/889,327 priority patent/US20250018697A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
    • B32B7/02—Physical, chemical or physicochemical properties
    • B32B7/023—Optical properties
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/06—Layered products comprising a layer of synthetic resin as the main or only constituent of a layer, which is next to another layer of the same or of a different material
    • B32B27/08—Layered products comprising a layer of synthetic resin as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/16—Layered products comprising a layer of synthetic resin specially treated, e.g. irradiated
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/28—Layered products comprising a layer of synthetic resin comprising synthetic resins not wholly covered by any one of the sub-groups B32B27/30 - B32B27/42
    • B32B27/281—Layered products comprising a layer of synthetic resin comprising synthetic resins not wholly covered by any one of the sub-groups B32B27/30 - B32B27/42 comprising polyimides
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/28—Layered products comprising a layer of synthetic resin comprising synthetic resins not wholly covered by any one of the sub-groups B32B27/30 - B32B27/42
    • B32B27/285—Layered products comprising a layer of synthetic resin comprising synthetic resins not wholly covered by any one of the sub-groups B32B27/30 - B32B27/42 comprising polyethers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/30—Layered products comprising a layer of synthetic resin comprising vinyl (co)polymers; comprising acrylic (co)polymers
    • B32B27/302—Layered products comprising a layer of synthetic resin comprising vinyl (co)polymers; comprising acrylic (co)polymers comprising aromatic vinyl (co)polymers, e.g. styrenic (co)polymers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/32—Layered products comprising a layer of synthetic resin comprising polyolefins
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/34—Layered products comprising a layer of synthetic resin comprising polyamides
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/36—Layered products comprising a layer of synthetic resin comprising polyesters
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/36—Layered products comprising a layer of synthetic resin comprising polyesters
    • B32B27/365—Layered products comprising a layer of synthetic resin comprising polyesters comprising polycarbonates
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B37/00—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding
    • B32B37/10—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding characterised by the pressing technique, e.g. using action of vacuum or fluid pressure
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B38/00—Ancillary operations in connection with laminating processes
    • B32B38/0008—Electrical discharge treatment, e.g. corona, plasma treatment; wave energy or particle radiation
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B9/00—Layered products comprising a layer of a particular substance not covered by groups B32B11/00 - B32B29/00
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F2/00—Processes of polymerisation
    • C08F2/46—Polymerisation initiated by wave energy or particle radiation
    • C08F2/48—Polymerisation initiated by wave energy or particle radiation by ultraviolet or visible light
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F2/00—Processes of polymerisation
    • C08F2/46—Polymerisation initiated by wave energy or particle radiation
    • C08F2/48—Polymerisation initiated by wave energy or particle radiation by ultraviolet or visible light
    • C08F2/50—Polymerisation initiated by wave energy or particle radiation by ultraviolet or visible light with sensitising agents
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F222/00—Copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by a carboxyl radical and containing at least one other carboxyl radical in the molecule; Salts, anhydrides, esters, amides, imides, or nitriles thereof
    • C08F222/10—Esters
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D135/00—Coating compositions based on homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by a carboxyl radical, and containing at least another carboxyl radical in the molecule, or of salts, anhydrides, esters, amides, imides or nitriles thereof; Coating compositions based on derivatives of such polymers
    • C09D135/02—Homopolymers or copolymers of esters
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D4/00—Coating compositions, e.g. paints, varnishes or lacquers, based on organic non-macromolecular compounds having at least one polymerisable carbon-to-carbon unsaturated bond ; Coating compositions, based on monomers of macromolecular compounds of groups C09D183/00 - C09D183/16
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/40—Oxides
    • C23C16/401—Oxides containing silicon
    • C23C16/402—Silicon dioxide
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/42—Silicides
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/44—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating
    • C23C16/50—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating using electric discharges
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2250/00—Layers arrangement
    • B32B2250/02—2 layers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2250/00—Layers arrangement
    • B32B2250/24—All layers being polymeric
    • B32B2250/244—All polymers belonging to those covered by group B32B27/36
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2255/00—Coating on the layer surface
    • B32B2255/10—Coating on the layer surface on synthetic resin layer or on natural or synthetic rubber layer
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2255/00—Coating on the layer surface
    • B32B2255/20—Inorganic coating
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2255/00—Coating on the layer surface
    • B32B2255/26—Polymeric coating
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2255/00—Coating on the layer surface
    • B32B2255/28—Multiple coating on one surface
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2307/00—Properties of the layers or laminate
    • B32B2307/70—Other properties
    • B32B2307/732—Dimensional properties
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2457/00—Electrical equipment
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B37/00—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding
    • B32B37/14—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding characterised by the properties of the layers
    • B32B37/16—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding characterised by the properties of the layers with all layers existing as coherent layers before laminating
    • B32B37/20—Methods or apparatus for laminating, e.g. by curing or by ultrasonic bonding characterised by the properties of the layers with all layers existing as coherent layers before laminating involving the assembly of continuous webs only

Definitions

  • the present disclosure relates to a laminate and a method for manufacturing the laminate.
  • JP 2019-119086 discloses a method in which a metal oxide film is formed on the surface of a base material by sputtering to form a laminate, and the metal oxide films of two laminates are bonded together. . According to the above method, since there is no need to use an adhesive or the like, the thickness of the resulting laminate can be reduced, and manufacturing costs can be reduced.
  • a problem to be solved by an embodiment of the present disclosure is to provide a laminate with excellent interlayer adhesion and a method for manufacturing the laminate.
  • the present disclosure includes the following aspects.
  • ⁇ 1> Comprising a first resin layer, an inorganic layer, and a second resin layer, and between the first resin layer and the inorganic layer, and between the second resin layer and the inorganic layer.
  • ⁇ 2> The laminate according to ⁇ 1> above, wherein the inorganic layer is a continuous layer.
  • ⁇ 3> The laminate according to ⁇ 1> or ⁇ 2> above, wherein the inorganic layer has a porosity of 25% or less.
  • ⁇ 4> The laminate according to any one of ⁇ 1> to ⁇ 3> above, wherein the mixed layer has a thickness of 1 nm to 30 nm.
  • ⁇ 5> Any one of ⁇ 1> to ⁇ 4> above, wherein the inorganic layer contains one or more inorganic materials selected from the group consisting of silicon oxide, silicon nitride, aluminum oxide, and aluminum nitride. 1.
  • ⁇ 6> The laminate according to any one of ⁇ 1> to ⁇ 5> above, wherein the inorganic layer contains silicon dioxide.
  • ⁇ 7> The laminate according to any one of ⁇ 1> to ⁇ 6> above, wherein the inorganic layer has a thickness of 5 nm or less.
  • ⁇ 9> Form a mixed layer and an inorganic layer in this order on the surfaces of each of the first resin layer and the second resin layer by plasma chemical vapor deposition, and a step of obtaining a first laminate comprising a layer, a second laminate comprising the second resin layer, the mixed layer and the inorganic layer; laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate;
  • a method for manufacturing a laminate including: ⁇ 10> The above, wherein the formation of the mixed layer and the inorganic layer on the first resin layer and the second resin layer, and the lamination of the first laminate and the second laminate are performed simultaneously. The method for manufacturing a laminate according to ⁇ 9>.
  • ⁇ 11> The laminate according to ⁇ 9> or ⁇ 10> above, wherein the inorganic layer of the first laminate and the inorganic layer of the second laminate have a surface roughness Ra of 2 nm or less. manufacturing method.
  • ⁇ 12> A first laminate comprising the first resin layer and the contrast layer, wherein a contrast layer is formed on each surface of the first resin layer and the second resin layer by a plasma chemical vapor deposition method.
  • a method for manufacturing a laminate including: ⁇ 13> In ⁇ 9> above, the formation of the contrast layer on the first resin layer and the second resin layer and the lamination of the first laminate and the second laminate are performed simultaneously.
  • FIG. 1 is a schematic cross-sectional view showing one embodiment of a laminate according to the first embodiment.
  • FIG. 2 is a schematic cross-sectional view showing one embodiment of the laminate according to the first embodiment.
  • FIG. 3 is a schematic diagram showing an embodiment of an apparatus that can be used to manufacture the laminate according to the first embodiment and the laminate according to the second embodiment.
  • FIG. 4 is a schematic diagram showing an embodiment of an apparatus that can be used to manufacture the laminate according to the first embodiment and the laminate according to the second embodiment.
  • FIG. 5 is a schematic diagram showing one embodiment of an apparatus that can be used to manufacture the laminate according to the first embodiment and the laminate according to the second embodiment.
  • a numerical range indicated using “ ⁇ ” indicates a range that includes the numerical value written before “ ⁇ ” as the lower limit value and the numerical value written before “ ⁇ ” as the upper limit value.
  • the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described step by step.
  • the upper limit or lower limit described in a certain numerical range may be replaced with the value shown in the Examples.
  • each component may contain multiple types of corresponding substances. If there are multiple types of substances corresponding to each component in the composition, the content rate or content of each component is the total content rate or content of the multiple types of substances present in the composition, unless otherwise specified. means quantity.
  • the term “layer” or “film” refers to the case where the layer or film is formed only in a part of the region, in addition to the case where the layer or film is formed in the entire region when observing the region where the layer or film is present. This also includes cases where it is formed.
  • laminate refers to stacking layers, and two or more layers may be bonded, or two or more layers may be removable.
  • (meth)acryloyl group means at least one of an acryloyl group and a methacryloyl group
  • (meth)acrylic means at least one of acrylic and methacrylic
  • step includes not only independent steps but also steps that cannot be clearly distinguished from other steps if the intended purpose is achieved.
  • the thickness of each layer is measured from a cross-sectional image obtained by a method for confirming the presence of a mixed layer, which will be described later.
  • the laminate 10 according to the first embodiment includes a first resin layer 11, an inorganic layer 12, and a second resin layer 13.
  • a mixed layer 14 is provided between the second resin layer 13 and the inorganic layer 12 and between the second resin layer 13 and the inorganic layer 12 .
  • the laminate 10 according to the first embodiment may include a support 15 on its outermost surface.
  • the laminate according to the first embodiment has excellent interlayer adhesion.
  • the reason why the first laminate has the above effect is not clear, but it is speculated as follows.
  • the laminate according to the first embodiment includes a mixed layer in which materials constituting these layers are mixed between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer. It is assumed that the mixed layer has excellent adhesion with the first resin layer and the inorganic layer, and excellent adhesion with the second resin layer and the inorganic layer, so that the adhesion between the layers is improved.
  • first resin layer, mixed layer, inorganic layer, mixed layer, and second resin layer of the laminate according to the first embodiment are provided continuously.
  • continuous provided means that there is no other layer between the layers (ie, there is no interface).
  • the laminate 20 according to the first embodiment includes a mixed layer 23, an inorganic layer 24, a mixed layer 23, and a third resin layer 25 on the surface of the second resin layer 22. It's okay. Further, a structure including a mixed layer, an inorganic layer, a mixed layer, and an n-th resin layer may be repeatedly provided on the surface of the third resin layer (not shown).
  • the first resin layer is indicated by the reference numeral 21, and the support body is indicated by the reference numeral 26.
  • the first resin layer and the second resin layer are made of epoxy resin, (meth)acrylic resin, liquid crystal polymer, polyester resin, polystyrene resin, fluororesin, polyimide resin, polyamide. It can contain resins such as polyamideimide resin, polyetherimide resin, cellulose resin, polyurethane resin, polyetherketone resin, and polycarbonate resin. Further, the resin layer may contain a reaction product of a (meth)acrylic monomer and a photopolymerization initiator. The resin layer may have a single layer structure or a multilayer structure. When the resin layer has a multilayer structure, the structure of each layer may be the same or different.
  • (meth)acrylic monomer those represented by the following general formula can be used.
  • R 1 represents a substituent, and each may be the same or different.
  • k represents an integer from 0 to 5, and may be the same or different. However, at least one of R 1 contains a polymerizable group.
  • R 2 is preferably a hydrogen atom or a hydroxy group. From the viewpoint of curability, it is preferable that at least one R 1 contains a hydroxy group.
  • the molecular weight of at least one R 1 is preferably from 10 to 250, more preferably from 70 to 150.
  • the bonding position of R 1 is preferably the para position.
  • k represents an integer of 0 to 5, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably both.
  • R 1 In the compound represented by the above general formula, it is preferable that at least two of R 1 have the same structure. Further, it is more preferable that all n is 1 and two of the four R 1s have the same structure, and it is even more preferable that all n is 1 and the four R 1s have the same structure. .
  • the polymerizable group is preferably a (meth)acryloyl group or an epoxy group, more preferably a (meth)acryloyl group.
  • the number of polymerizable groups is preferably two or more, more preferably three or more. Moreover, although the upper limit of the number of polymerizable groups is not particularly determined, it is preferably 8 or less, and more preferably 6 or less.
  • the molecular weight of the compound represented by the above general formula is preferably 600 to 1,400, more preferably 800 to 1,200.
  • n represents an integer of 0 to 5, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 1.
  • photopolymerization initiator conventionally known ones can be used, including ⁇ -carbonyl compounds, acyloin ether compounds, ⁇ -hydrocarbon-substituted aromatic acyloin compounds, polynuclear quinone compounds, triarylimidazole dimers and p-amino Examples include combinations with phenyl ketones, acridine compounds, phenazine compounds, oxadiazole compounds, and acylphosphine oxide compounds.
  • the content of the resin with respect to the total mass of the resin layer is not particularly limited, and may be 50% by mass to 100% by mass, 70% by mass to 95% by mass, or 80% by mass to It may be 90% by mass.
  • the resin layer may contain additives such as pigments, dyes, ultraviolet absorbers, light stabilizers, antioxidants, and waxes.
  • the thickness of the resin layer is preferably 0.05 ⁇ m to 50 ⁇ m, more preferably 0.1 ⁇ m to 20 ⁇ m, and even more preferably 0.5 ⁇ m to 10 ⁇ m.
  • the materials such as resin contained in the first resin layer and the second resin layer may be the same or different.
  • the thickness of the first resin layer and the second resin layer may be the same or different.
  • the laminate according to the first embodiment further includes a resin layer (a third resin layer, a fourth resin layer, etc.) in addition to the first resin layer and the second resin layer, The material and thickness of these resin layers may be the same as or different from those of the first resin layer and the second resin layer.
  • the resin layer can be formed by applying a resin composition containing the above resin etc. to the surface of the support and drying it. Further, after drying, it may be irradiated with ultraviolet rays, electron beams, etc. to be photocured.
  • the inorganic layer can contain an inorganic material, and examples of the inorganic material include inorganic oxides, inorganic nitrides, metal oxides, and metal nitrides.
  • examples of inorganic oxides include silicon oxides and boron oxides.
  • examples of the inorganic nitride include silicon nitride, boron nitride, and the like.
  • Examples of metal oxides include aluminum oxide, titanium oxide, iron oxide, copper oxide, chromium oxide, magnesium oxide, zirconium oxide, and the like.
  • the inorganic layer preferably contains one or more inorganic materials selected from the group consisting of silicon oxide, silicon nitride, aluminum oxide, and aluminum nitride, It is more preferable to contain one or more inorganic materials selected from the group consisting of silicon oxides and silicon nitrides. From the viewpoint of interlayer adhesion, the inorganic layer preferably contains silicon oxide, and more preferably contains silicon dioxide.
  • the content of the inorganic material with respect to the total mass of the inorganic layer is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 95% by mass, and 80% by mass. % to 90% by mass is more preferable.
  • the inorganic layer is a continuous layer.
  • a continuous layer means a layer in which the porosity within the inorganic layer is 50% or less. Note that in the present disclosure, voids do not include defects. From the viewpoint of interlayer adhesion, the porosity of the inorganic layer is preferably 25% or less, more preferably 10% or less. The lower limit of the porosity of the inorganic layer is not particularly limited, and may be 0%.
  • porosity is measured as follows. First, a cross-sectional image obtained by a method for confirming the presence of a mixed layer, which will be described later, is prepared. In the inorganic layer forming part of the above cross-sectional image, the area S0 of the part where the density is 0 to 50 and the length in the thickness direction is 2 nm or more is determined, and divided by the area S1 of the entire inorganic layer forming part, The porosity of the inorganic layer is determined by multiplying by 100. Note that even if the concentration is between 0 and 50, if the length in the thickness direction is less than 2 nm, it is not considered as a void.
  • the material and thickness of each inorganic layer may be the same or different.
  • the thickness of the inorganic layer is preferably 30 nm or less, more preferably 28 nm or less, even more preferably 23 nm or less, and particularly preferably 5 nm or less. Further, by setting the thickness of the inorganic layer to 30 nm or less, it is possible to suppress a decrease in adhesion between the layers due to bending the laminate or applying force. From the viewpoint of interlayer adhesion, the thickness of the inorganic layer is preferably 1 nm or more, more preferably 2 nm or more.
  • the thickness of the inorganic layer is preferably 1 nm to 30 nm, more preferably 1 nm to 28 nm, even more preferably 1 nm to 23 nm, and particularly preferably 2 nm to 5 nm.
  • the thickness of the inorganic layer can be determined by changing the feeding speed of the resin layer, the flow rate of the raw materials and oxygen gas used to form the inorganic layer and the mixed layer, the peak voltage, etc. in the method for manufacturing the laminate described below. Can be adjusted.
  • the laminate according to the first embodiment includes a mixed layer between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer.
  • the mixed layer is a layer formed when forming an inorganic layer on the surface of the first resin layer or the second resin layer, and its existence is confirmed by the following method.
  • the laminate according to the first embodiment is cut out into a size of 3 mm in length x 3 mm in width, and is used as a test piece A. Test piece A is placed in a transmission electron microscope, and the cross section of the test piece in the thickness direction is irradiated with an electron beam for 10 minutes at a voltage of 300 kV.
  • a cross-sectional image (magnification: 1,000,000 times) of test piece A after electron beam irradiation is acquired.
  • the density of the cross-sectional image is measured using image analysis software.
  • the density of the highest density part (inorganic layer part) in the above cross-sectional image is 100, and the density of the lowest density part (first resin layer part and second resin layer part) is 0, the inorganic layer
  • the presence of a portion with a concentration of 10 to 90 between the resin layer and the resin layer (in the thickness direction) is confirmed, and if confirmed, it is determined that a mixed layer exists.
  • the test piece A is embedded in a molten resin, the resin is then irradiated with light and cured to obtain a cured product A, and the cured product A is cut out to a thickness of 20 nm lengthwise, and a test piece B Then, the cross section of this test piece B in the thickness direction may be irradiated with an electron beam.
  • the transmission electron microscope JEM-2011 manufactured by JEOL Ltd. or a device equivalent to this can be used.
  • the density in the cross-sectional image is confirmed using image analysis software Image J or similar software.
  • trimethylolpropane triacrylate can be used as the resin.
  • the mixed layer preferably contains a resin contained in the resin layer and an inorganic material contained in the inorganic layer.
  • the content of the resin relative to the total mass of the mixed layer is preferably 5% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and 30% by mass. More preferably, it is 70% by mass.
  • the content of the inorganic material with respect to the total mass of the mixed layer is preferably 10% by mass to 95% by mass, more preferably 20% by mass to 80% by mass, and 30% by mass. % to 70% by mass is more preferable.
  • the thickness of the mixed layer is preferably 1 nm to 30 nm, and 2 nm to 2 nm. It is more preferably 25 nm to 25 nm, even more preferably 2 nm to 20 nm, and particularly preferably 3 nm to 15 nm.
  • the thickness of the mixed layer can be determined by changing the feeding speed of the resin layer, the flow rate of the raw materials and oxygen gas used to form the inorganic layer and the mixed layer, the peak voltage, etc. in the method for manufacturing the laminate described below. Can be adjusted.
  • the support can contain resins such as polyester resins, polyolefin resins, polystyrene resins, polyamide resins, polycarbonate resins, polyimide resins, polyamideimide resins, (meth)acrylic resins, and the like. Moreover, the support can contain the above-mentioned additives.
  • the support may have a single layer structure or a multilayer structure. When the support has a multilayer structure, the structure of each layer may be the same or different.
  • the thickness of the support is not particularly limited, and can be, for example, 10 ⁇ m to 500 ⁇ m.
  • the support one manufactured by a conventionally known method may be used, or one that is commercially available may be used.
  • the laminate according to the first embodiment can be manufactured by a method for manufacturing a laminate according to the first embodiment described below.
  • the laminate according to the second embodiment is a laminate including a first resin layer and a second resin layer, A contrast layer containing an inorganic material is provided between the first resin layer and the second resin layer, A cross-section of the laminate was irradiated with an electron beam for 10 minutes using a transmission electron microscope at a voltage of 300 kV, and a cross-sectional image of the test piece after electron beam irradiation was obtained. Toward this end, the density measured by image analysis software decreases.
  • the "surface" of the contrast layer refers to a range of 2 nm from the surface in the thickness direction. Furthermore, in the present disclosure, the inside of the contrast layer refers to a portion other than the surface of the contrast layer.
  • the laminate according to the second embodiment may include a support on its outermost surface.
  • the laminate according to the second embodiment may further include a contrast layer and a third resin layer on the surface of the second resin layer. Further, a structure consisting of a contrast layer and an n-th resin layer may be repeatedly provided on the surface of the third resin layer.
  • the resin layer and support are the same as those of the laminate according to the first embodiment, so their description will be omitted here.
  • the laminate according to the second embodiment includes a contrast layer between the resin layers.
  • the contrast layer refers to a layer in which the density measured by image analysis software decreases from the inside of the contrast layer toward the surface in a cross-sectional image obtained by a transmission electron microscope.
  • the presence of the contrast layer is confirmed as follows.
  • the laminate according to the second embodiment was cut out into a size of 3 mm in length x 3 mm in width, and used as a test piece a.
  • Test piece a is placed in a transmission electron microscope, and the cross section of the test piece in the thickness direction is irradiated with an electron beam for 10 minutes at a voltage of 300 kV.
  • a cross-sectional image (1,000,000 times magnification) of the test piece a after electron beam irradiation is acquired.
  • the density data of the contrast layer is obtained from the cross-sectional image, and it is confirmed whether the density decreases from the inside of the contrast layer toward the surface.
  • the test piece a is embedded in a molten resin, the resin is then irradiated with light and cured to obtain a cured product a, and the cured product a is cut out to a thickness of 20 nm lengthwise, and the test piece b is Then, an electron beam may be irradiated onto the cross section of the test piece b in the thickness direction.
  • the transmission electron microscope JEM-2011 manufactured by JEOL Ltd. or a device equivalent to this can be used.
  • the density in the cross-sectional image is confirmed using image analysis software Image J or similar software.
  • trimethylolpropane triacrylate can be used as the resin.
  • the contrast layer has a density of 3 to 50 per nm from the inside to the surface.
  • the concentration of 10 to 35 is reduced, more preferably 10 to 35.
  • the contrast layer is a layer formed when an inorganic layer is formed on the surface of the first resin layer or the second resin layer, and may include the above-described inorganic layer and a mixed layer. It may also include only Since the inorganic layer and the mixed layer have been described above, their description will be omitted here.
  • the thickness of the contrast layer is preferably 1 nm to 30 nm, more preferably 2 nm to 20 nm, even more preferably 2 nm to 15 nm, and even more preferably 2 nm to 10 nm. is particularly preferred.
  • the laminate according to the second embodiment can be manufactured by a laminate manufacturing method described below.
  • the laminate according to the first embodiment and the laminate according to the second embodiment are applicable to electronic devices such as organic EL (elactor luminescence) displays, organic EL lighting, organic solar cells, CIGS (copper indium gallium selenide) solar cells, It can be applied to optical devices such as AR glasses.
  • organic EL epilactor luminescence
  • organic solar cells organic solar cells
  • CIGS copper indium gallium selenide
  • the method for manufacturing a laminate according to the first embodiment includes forming a mixed layer and an inorganic layer in this order on each surface of a first resin layer and a second resin layer by a plasma chemical vapor deposition method; A step of obtaining a first laminate comprising a resin layer, a mixed layer and an inorganic layer, and a second laminate comprising a second resin layer, a mixed layer and an inorganic layer (hereinafter, forming a mixed layer and an inorganic layer) ) and A step of laminating an inorganic layer of a first laminate and an inorganic layer of a second laminate (hereinafter also referred to as a lamination step); including.
  • a laminate with excellent interlayer adhesion can be manufactured.
  • a mixed layer is formed by forming an inorganic layer on the first resin layer and the second resin layer by plasma chemical vapor deposition. This is because the surfaces of the first resin layer and the second resin layer are etched by plasma chemical vapor deposition, and an inorganic material to form an inorganic layer enters the etched parts, so that a mixed layer is formed. I guess.
  • the mixed layer has excellent adhesion with the first resin layer and the inorganic layer, and excellent adhesion with the second resin layer and the inorganic layer, and the inorganic layer formed by plasma chemical vapor deposition has Since the surface is activated and the inorganic layers are laminated together, the adhesion between the inorganic layers is excellent. Therefore, the adhesion between the layers of the laminate manufactured by the method for manufacturing the laminate according to the first embodiment is Guess it's better.
  • the step of forming a mixed layer and an inorganic layer, and the step of laminating may be repeated multiple times.
  • the second resin layer and the separately prepared third resin layer of the manufactured laminate are coated by plasma chemical vapor deposition.
  • a third laminate comprising a mixed layer and an inorganic layer formed in this order, a first resin layer, a mixed layer, an inorganic layer, a mixed layer, a second resin layer, a mixed layer and an inorganic layer, and a third resin a fourth laminate comprising a layer, a mixed layer and an inorganic layer;
  • the method may include a step of laminating an inorganic layer provided on the outermost surface of the third laminate and an inorganic layer of the fourth laminate.
  • the method for manufacturing the laminate according to the first embodiment includes forming a mixed layer and A step of forming inorganic layers in this order to obtain a first laminate including a first resin layer, a mixed layer, and an inorganic layer, and a second laminate including a second resin layer, a mixed layer, and an inorganic layer. including.
  • the details of the first resin layer, second resin layer, mixed layer, and inorganic layer have been described above, so their description will be omitted here.
  • the mixed layer and the inorganic layer are formed on the resin layer by plasma chemical vapor deposition. More specifically, an oxygen gas containing raw materials for forming an inorganic layer such as silane and a mixed layer is brought into a plasma state using plasma excitation power, and the surface of the resin layer is plasma-treated using the plasma-stated oxygen gas.
  • the method allows the formation of mixed layers and inorganic layers. Examples of the plasma treatment method include a method in which the surface of the resin layer is irradiated with plasma using a plasma irradiation device, a method in which the resin layer is passed between an electrode roller and a support roller in the oxygen gas atmosphere, and the like. .
  • oxygen gas containing raw materials hydrogen gas, gas containing nitrogen atoms, inert gas, etc. may be used.
  • gas containing nitrogen atoms include nitrogen gas (N 2 ), ammonia gas (NH 3 ), nitrous oxide gas (N 2 O), and the like.
  • inert gas include helium gas, neon gas, argon gas, krypton gas, xenon gas, and radon gas.
  • the flow rate of oxygen gas is preferably 30 mL/min to 350 mL/min, and 40 mL/min to 300 mL/min. More preferably, it is 50 mL/min to 250 mL/min.
  • the flow rate of the raw material is preferably 2 mg/min to 17 mg/min, and preferably 3 mg/min to 15 mg/min. More preferably, the amount is 4 mg/min to 10 mg/min.
  • the peak voltage of the plasma excitation power used in plasma generation of the raw material gas to form a mixed layer and an inorganic layer on the surface of the resin layer and to improve interlayer adhesion is 3 kV to 17 kV. It is preferably 4 kV to 15 kV, and even more preferably 6 kV to 10 kV.
  • peak voltage of plasma excitation power means the maximum value of plasma excitation power during plasmaization of source gas.
  • the method of laminating the first laminate and the second laminate is not particularly limited, and the inorganic layer of the first laminate and the inorganic layer of the second laminate are faced to each other. This may also be done by crimping.
  • the laminates may be pressed together by overlapping the laminates and passing them between rollers.
  • the pressure applied to the laminate by the roller is not particularly limited, and can be, for example, 0.1 MPa to 5 MPa.
  • the method for manufacturing a laminate according to the first embodiment includes forming a mixed layer and an inorganic layer on a first resin layer and a second resin layer, and laminating the first laminate and the second laminate. It is preferable to do both at the same time. As a result, unevenness is formed on the surface of the resin layer by etching, and the material forming the inorganic layer penetrates into the uneven part, and the lamination of the inorganic layers of the laminate is performed simultaneously, so the inorganic layer to be laminated is The smoothness of the interface between the layers tends to improve, and the adhesion between the layers tends to improve.
  • the surface roughness Ra of the inorganic layer of the first laminate and the inorganic layer of the second laminate is preferably 2 nm or less, more preferably 1.5 nm or less. preferable.
  • the lower limit of the surface roughness is not particularly limited, and can be, for example, 0.3 nm or more. Note that in the present disclosure, the surface roughness Ra is measured based on "JIS B 0601 (2013)".
  • the measurement device is AFM (manufactured by Hitachi High-Technology Co., Ltd., SPA400) or an equivalent device.
  • FIG. 3 shows an embodiment of an apparatus that can be used in the method for manufacturing a laminate according to the first embodiment.
  • the device 30 shown in FIG. 3 includes an unwinding roller 33 for feeding out the first resin layer 31 and the second resin layer 32.
  • the first resin layer 31 and the second resin layer 32 may be formed on the surface of the support, respectively, and a laminate including the support and the resin layer may be unwound.
  • the apparatus 30 also applies plasma to form a mixed layer and an inorganic layer on the surfaces of the first resin layer 31 and the second resin layer 32 to form a first laminate and a second laminate.
  • a plasma irradiation device 34 for irradiation is provided.
  • the device 30 also includes a pressure roller 35 for laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate.
  • the device 30 also includes a roller 36 (take-up roller) that winds up a laminate obtained by laminating the first laminate and the second laminate using a pressure roller.
  • the formation of the mixed layer and the inorganic layer on the first resin layer and the second resin layer and the lamination of the first laminate and the second laminate can be performed simultaneously. First, the first resin layer 31 and the second resin layer 32 are fed out by the feeding roller 33 .
  • the plasma irradiation device 34 irradiates plasma toward the joint portion of the pressure roller 35 to form a mixed layer and an inorganic layer on the surfaces of the first resin layer 31 and the second resin layer 32. While obtaining the first laminate and the second laminate, the inorganic layer of the first laminate and the inorganic layer of the second laminate are laminated.
  • FIG. 4 shows another embodiment of an apparatus that can be used in the method for manufacturing a laminate according to the first embodiment.
  • the first laminate and the second laminate are laminated after forming the mixed layer and the inorganic layer on the first resin layer and the second resin layer.
  • the first resin layer is denoted by 41
  • the second resin layer is denoted by 42
  • the unwinding roller is denoted by 43
  • the plasma irradiation device is denoted by 44
  • the pressure roller is denoted by 45
  • the winding roller is denoted by 47.
  • FIG. 5 shows still another embodiment of the apparatus that can be used in the method for manufacturing a laminate according to the first embodiment.
  • the device 50 shown in FIG. 5 includes an electrode roller 56 and a support roller 57, and between these rollers, oxygen gas containing raw materials is turned into plasma, and a mixed layer and a mixed layer are formed on the surfaces of the first resin layer and the second resin layer. An inorganic layer can be formed.
  • the device 50 shown in FIG. 5 may include a casing 58 for filling the oxygen gas and a nozzle (not shown) for introducing the oxygen gas between the electrode roller 56 and the support roller 57.
  • the first resin layer is indicated by reference numeral 51
  • the second resin layer is indicated by reference numeral 52
  • the unwinding roller is indicated by reference numeral 53
  • the pressure roller is indicated by reference numeral 54
  • the winding roller is indicated by reference 55.
  • the method for manufacturing a laminate according to the second embodiment includes forming a contrast layer on each surface of the first resin layer and the second resin layer by a plasma chemical vapor deposition method, and forming a contrast layer on each surface of the first resin layer and the second resin layer.
  • a step of obtaining a first laminate including a layer and a second laminate including a second resin layer and a contrast layer (hereinafter also referred to as a step of forming a contrast layer);
  • a step of laminating a contrast layer of a first laminate and a contrast layer of a second laminate (hereinafter also referred to as a lamination step); including.
  • the step of forming a contrast layer and the step of laminating may be repeated multiple times.
  • the second resin layer and the separately prepared third resin layer of the manufactured laminate are coated on each surface by plasma chemical vapor deposition.
  • a contrast layer is formed to obtain a third laminate including a first resin layer, a contrast layer, a second resin layer, and a contrast layer, and a fourth laminate including a third resin layer and a contrast layer.
  • process and a step of laminating a contrast layer provided on the outermost surface of the third laminate and a contrast layer of the fourth laminate can include.
  • the method for manufacturing a laminate according to the second embodiment includes forming a contrast layer on each surface of the first resin layer and the second resin layer by a plasma chemical vapor deposition method, and forming a contrast layer on each surface of the first resin layer and the second resin layer. obtaining a first laminate comprising a layer and a second laminate comprising a second resin layer and a contrast layer.
  • the details of the first resin layer, the second resin layer, and the contrast layer have been described above, so their description will be omitted here.
  • the contrast layer is formed on the resin layer by plasma chemical vapor deposition. More specifically, a contrast layer is formed by a method in which a mixture of raw material gas such as silane and oxygen gas is brought into a plasma state using excitation power, and the surface of the resin layer is plasma-treated using the plasma-stated gas. can do.
  • the contrast layer is formed when the rate of etching the surface of the resin layer is higher than the rate of formation of the inorganic layer on the surface of the resin layer.
  • the formation rate of the inorganic layer can be adjusted by changing the flow rates of oxygen gas and raw materials.
  • the etching rate can be adjusted by changing the peak voltage.
  • Examples of the plasma treatment method include a method in which the surface of the resin layer is irradiated with plasma using a plasma irradiation device, a method in which the resin layer is passed between an electrode roller and a support roller in the oxygen gas atmosphere, and the like. .
  • hydrogen gas gas containing nitrogen atoms
  • inert gas gas containing nitrogen atoms
  • gas containing nitrogen atoms include nitrogen gas (N 2 ), ammonia gas (NH 3 ), nitrous oxide gas (N 2 O), and the like.
  • inert gas include helium gas, neon gas, argon gas, krypton gas, xenon gas, and radon gas.
  • the flow rate of oxygen gas is preferably 30 mL/min to 350 mL/min, and preferably 40 mL/min to 300 mL/min. is more preferable, and even more preferably 50 mL/min to 250 mL/min.
  • the flow rate of oxygen gas is preferably 5 mL/min to 28 mL/min, and 6 mL/min to 25 mL. It is more preferable that it is 7 mL/min to 23 mL/min.
  • the flow rate of the raw material is preferably 2 mg/min to 17 mg/min, and preferably 3 mg/min to 15 mg/min. More preferably, the amount is 4 mg/min to 10 mg/min.
  • the flow rate of the raw material is preferably 0.1 mg/min to 1.8 mg/min, and 0.1 mg/min to 1.8 mg/min. More preferably, the amount is 3 mg/min to 1.5 mg/min, and even more preferably 0.5 mg/min to 1.3 mg/min.
  • the peak voltage of the plasma excitation power used in plasma generation of the raw material gas to form a contrast layer on the surface of the resin layer and improve interlayer adhesion is preferably 3 kV to 17 kV. , more preferably 4 kV to 15 kV, even more preferably 6 kV to 10 kV.
  • the method of laminating the first laminate and the second laminate is not particularly limited, and the contrast layer of the first laminate and the contrast layer of the second laminate are placed facing each other. This may also be done by crimping.
  • the laminates may be pressed together by overlapping the laminates and passing them between rollers.
  • the pressure applied to the laminate by the roller is not particularly limited, and can be, for example, 0.1 MPa to 5 MPa.
  • forming a contrast layer on the first resin layer and the second resin layer and laminating the first laminate and the second laminate are performed simultaneously. It is preferable to do so.
  • unevenness is formed on the surface of the resin layer by etching, and the material forming the contrast layer penetrates into the uneven portion, and the contrast layers of the laminate are laminated simultaneously, so the contrast layer to be laminated is The smoothness of the interface between the layers tends to improve, and the adhesion between the layers tends to improve.
  • the surface roughness of the contrast layer of the first laminate and the contrast layer of the second laminate is preferably 2 nm or less, more preferably 1.5 nm or less. .
  • the apparatus that can be used in the method for manufacturing a laminate according to the first embodiment can also be used in the method for manufacturing a laminate according to the second embodiment.
  • Example 1 Two polyethylene terephthalate films (manufactured by Toyobo Co., Ltd., A4100) each having a thickness of 100 ⁇ m and a width of 50 mm were prepared as supports. A resin composition having the following composition was applied to one surface of each support, dried, and photocured to form a first resin layer and a second resin layer with a thickness of 2 ⁇ m.
  • Composition of resin composition ⁇ Acrylic monomer (manufactured by Shin Nakamura Chemical Co., Ltd., TMPTA) 95.5% by mass
  • Photopolymerization initiator manufactured by Lamberti, KTO46
  • An apparatus 30 shown in FIG. 3 was prepared.
  • a laminate including a support and a first resin layer and a laminate including a support and a second resin layer were conveyed from each of the unwinding rollers 33 at a speed of 1 m/min.
  • Plasma is irradiated from the below-described plasma irradiation device 34 under the following conditions toward the joint location of the pressure roller 35 provided in the device 30, thereby forming a mixed layer and an inorganic layer ( 5 nm) to form a first laminate and a second laminate, and laminate the inorganic layer (silicon dioxide) of the first laminate and the inorganic layer (silicon dioxide) of the second laminate.
  • a laminate was obtained. Note that the pressure applied to the laminate by the pressure roller was 0.2 MPa.
  • the thickness of the inorganic layer in the laminate was 10 nm.
  • the first laminate and the second laminate were prepared under the same conditions as described above.
  • the surface roughness Ra of the inorganic layer of each laminate was measured using an AFM (manufactured by Hitachi High-Tech Corporation, SPA400) based on "JIS B 0601 (2013)", and both were 0.9 nm. there were.
  • test piece A The laminate produced as described above was cut out into a size of 3 mm in length x 3 mm in width to obtain test piece A.
  • the above test piece A was embedded in molten trimethylolpropane triacrylate, then irradiated with light to form a cured product A (thickness 200 ⁇ m, length 5 mm, width 10 mm).
  • the sample was cut out and designated as a test piece B, and the cross section of the test piece B in the thickness direction was irradiated with an electron beam for 10 minutes at a voltage of 300 kV.
  • a cross-sectional image (magnification: 1,000,000 times) of test piece B after electron beam irradiation was obtained.
  • the density of the cross-sectional image was measured using image analysis software.
  • the inorganic layer part When the density of the highest density part (inorganic layer part) in the above cross-sectional image is 100, and the density of the lowest density part (first resin layer part and second resin layer part) is 0, the inorganic layer It was confirmed that there were parts with a concentration of 10 to 90 between the inorganic layer and the first resin layer, and between the inorganic layer and the second resin layer. Note that as a transmission electron microscope, JEM-2011 manufactured by JEOL Ltd. was used. In addition, the density in the cross-sectional image was confirmed using image analysis software Image J. The thicknesses of the inorganic layer and the mixed layer of the laminate were measured from the cross-sectional image and were 10 nm and 5 nm, respectively.
  • the area S0 of the part where the density is 0 to 50 and the length in the thickness direction is 2 nm or more is determined, and divided by the area S1 of the entire inorganic layer forming part, The porosity of the inorganic layer was determined by multiplying by 100 and was found to be less than 5%.
  • Example 2 A laminate was manufactured in the same manner as in Example 1 except that the peak voltage was changed to 6 kV. In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 9 nm and 2 nm, respectively. Further, when the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.9 nm.
  • Example 3 A laminate was manufactured in the same manner as in Example 1 except that the peak voltage was changed to 10 kV. In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 12 nm and 10 nm, respectively. Further, when the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 1.0 nm.
  • Example 4 A laminate was manufactured in the same manner as in Example 1 except that the peak voltage was changed to 15 kV. In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 14 nm and 28 nm, respectively. Further, when the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 1.2 nm.
  • Example 5 A laminate was produced in the same manner as in Example 1, except that the flow rates of tetraethoxysilane gas and oxygen gas were changed to 10 mg/min and 200 mL/min, respectively.
  • the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 22 nm and 5 nm, respectively.
  • the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%.
  • the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 1.3 nm.
  • Example 6> A laminate was produced in the same manner as in Example 1, except that the flow rates of tetraethoxysilane gas and oxygen gas were changed to 15 mg/min and 300 mL/min, respectively. In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 28 nm and 5 nm, respectively. Further, when the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 1.4 nm.
  • Example 7 A laminate was produced in the same manner as in Example 1, except that the flow rates of tetraethoxysilane gas and oxygen gas were changed to 2 g/min and 40 mL/min, respectively.
  • the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 4 nm and 5 nm, respectively.
  • the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%.
  • the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.8 nm.
  • Example 8> A laminate was produced in the same manner as in Example 1, except that trimethylaluminum was used instead of tetraethoxysilane. In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer (aluminum oxide) included in the laminate and the mixed layer were measured and found to be 10 nm and 4 nm, respectively. Further, when the porosity of the inorganic layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 1 nm.
  • a laminate manufacturing apparatus 40 shown in FIG. 4 was prepared.
  • a laminate including a support and a first resin layer and a laminate including a support and a second resin layer were conveyed from each of the unwinding rollers 43 at a speed of 1 m/min.
  • Plasma is irradiated from the following plasma irradiation device under the following conditions to form a mixed layer and an inorganic layer on the surfaces of the first resin layer and the second resin layer, and form the first laminate and the second laminate. Obtained.
  • the inorganic layer of the first laminate and the inorganic layer of the second laminate were laminated using the pressure roller 45 included in the device 40 to obtain a laminate. Note that the pressure applied to the laminate by the pressure roller was 0.2 MPa.
  • Example 2 In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 4 nm and 5 nm, respectively. Further, the porosity of the inorganic layer was determined in the same manner as in Example 1, and was found to be 25%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.8 nm.
  • Example 10 A laminate was produced in the same manner as in Example 9, except that the area from the plasma irradiation part to the pressure roller was surrounded by a casing, and the inside of the casing was made into a nitrogen atmosphere.
  • the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 4 nm and 5 nm, respectively.
  • the porosity of the inorganic layer was determined in the same manner as in Example 1, and was found to be 10%.
  • the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.8 nm.
  • Example 11 A laminate manufacturing apparatus 50 shown in FIG. 5 was prepared. A laminate including a support and a first resin layer and a laminate including a support and a second resin layer were conveyed from each of the unwinding rollers 53 at a speed of 1 m/min.
  • Tetraethoxysilane gas (flow rate: 5 mg/min), oxygen gas (flow rate: 100 mL/min), and nitrogen gas (flow rate: 500 mL/min) are introduced into the casing 58 from the nozzle, and the support and the first resin layer are A laminate comprising a support body and a second resin layer is passed between an electrode roller 56 and a support roller 57 provided in a casing 58, and the first resin layer and second resin layer are A mixed layer and an inorganic layer were formed on the surface to obtain a first laminate and a second laminate.
  • the inorganic layer of the first laminate and the inorganic layer of the second laminate were laminated using the pressure roller 54 included in the device 50 to obtain a laminate. Note that the pressure applied to the laminate by the pressure roller was 0.2 MPa.
  • Example 2 In the same manner as in Example 1, the presence of the mixed layer was confirmed, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured and found to be 3 nm and 6 nm, respectively. Further, the porosity of the inorganic layer was determined in the same manner as in Example 1, and was found to be 25%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.8 nm.
  • Example 1 Example except that a sputtering device was provided in place of the atmospheric pressure plasma jet device, and an inorganic layer (silicon dioxide) was formed on the surfaces of the first resin layer and the second resin layer by the sputtering method under the following conditions.
  • a laminate was produced in the same manner as in Example 1. (Conditions for sputtering method) ⁇ Argon flow rate: 100mL/min ⁇ Power: 200W ⁇ Frequency: 13.56MHz
  • the presence of the mixed layer was confirmed in the same manner as in Example 1, but the presence of the mixed layer was not confirmed. Furthermore, the thickness of the inorganic layer included in the laminate was measured and found to be 10 nm. Further, the porosity of the inorganic layer was determined in the same manner as in Example 1, and was found to be 27%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.7 nm.
  • ⁇ Adhesion evaluation-1> When forming the first resin layer on the surface of the support, a film with a width of 50 mm x length of 10 mm was sandwiched at the end of the support, and a portion was provided where the support and the first resin layer did not come into close contact. produced a laminate in the same manner as in the above Examples and Comparative Examples. The above laminate was cut into a size of 50 mm in the transport direction x 25 mm in the width direction to form a test piece, and the support on the second resin layer side was attached to the base with double-sided tape and fixed. Next, the non-adhering portion of the support that was in contact with the first resin layer of the test piece was folded back.
  • the folded portion was pulled in a 180° direction (peel speed: 5 mm/sec) using a peel tester (manufactured by Shimadzu Corporation, universal tester AGS-100NX), and the maximum load (N/25 mm) was measured.
  • peel tester manufactured by Shimadzu Corporation, universal tester AGS-100NX
  • maximum load N/25 mm
  • Adhesion evaluation-2> After performing the following bending test on the test piece prepared in Adhesion Evaluation-1, the maximum load (N/25 mm) was measured in the same manner as in Adhesion Evaluation-1, and the results are summarized in Table 1. One end of the test piece in the length direction was fixed. A rod with a diameter of 10 mm was placed in the center of the test piece, and using this as a fulcrum, one end of the test piece that was not fixed was bent by 180°, and then returned to its original position. The above bending was repeated 10,000 times.
  • Example 12 Two polyethylene terephthalate films (manufactured by Toyobo Co., Ltd., A4100) each having a thickness of 100 ⁇ m and a width of 50 mm were prepared as supports. A resin composition having the following composition was applied to one surface of each support, dried, and photocured to form a first resin layer and a second resin layer with a thickness of 2 ⁇ m.
  • Composition of resin composition ⁇ Acrylic monomer (manufactured by Shin Nakamura Chemical Co., Ltd., TMPTA) 95.5% by mass
  • Photopolymerization initiator manufactured by Lamberti, KTO46
  • An apparatus 30 shown in FIG. 3 was prepared.
  • a laminate including a support and a first resin layer and a laminate including a support and a second resin layer were conveyed from each of the unwinding rollers 33 at a speed of 1 m/min.
  • Plasma is irradiated from the below-described plasma irradiation device 34 under the following conditions toward the joint location of the pressure roller 35 provided in the device 30 to form a contrast layer on the surfaces of the first resin layer and the second resin layer, A first laminate and a second laminate were formed, and the contrast layer of the first laminate and the contrast layer of the second laminate were laminated to obtain a laminate.
  • the pressure applied to the laminate by the pressure roller was 0.2 MPa.
  • test piece a The laminate produced as described above was cut out into a size of 3 mm in length x 3 mm in width to form a test piece a.
  • the above test piece a was embedded in molten trimethylolpropane triacrylate, then irradiated with light to form a cured product b (thickness 200 ⁇ m, length 5 mm, width 10 mm). This was cut out to give a test piece b, and the cross section of the test piece b in the thickness direction was irradiated with an electron beam for 10 minutes at a voltage of 300 kV.
  • a cross-sectional image (magnification: 1,000,000 times) of test piece b after electron beam irradiation was obtained. The density of the cross-sectional image was measured using image analysis software.
  • the maximum density inside the contrast layer in the above cross-sectional image is 100 and the density of the first resin layer and the second resin layer is 0, the density decreases by 25 per nm from the inside of the contrast layer toward the surface. was confirmed. Further, when the porosity of the contrast layer was determined in the same manner as in Example 1, it was less than 5%. Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1, and was found to be 0.6 nm.
  • Adhesion Evaluation-1 and Adhesion Evaluation-2 were conducted in the same manner as in Example 1, and the maximum loads were both 12 N/25 mm.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Mechanical Engineering (AREA)
  • General Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Physics & Mathematics (AREA)
  • Polymers & Plastics (AREA)
  • Medicinal Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Plasma & Fusion (AREA)
  • Wood Science & Technology (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Fluid Mechanics (AREA)
  • Thermal Sciences (AREA)
  • Laminated Bodies (AREA)
PCT/JP2022/042287 2022-03-25 2022-11-14 積層体及び積層体の製造方法 Ceased WO2023181489A1 (ja)

Priority Applications (5)

Application Number Priority Date Filing Date Title
EP22933619.3A EP4501621A4 (en) 2022-03-25 2022-11-14 Laminate and method for producing laminate
KR1020247030376A KR20240151785A (ko) 2022-03-25 2022-11-14 적층체 및 적층체의 제조 방법
JP2024509737A JPWO2023181489A1 (cg-RX-API-DMAC7.html) 2022-03-25 2022-11-14
CN202280093717.8A CN118900765A (zh) 2022-03-25 2022-11-14 层叠体及层叠体的制造方法
US18/889,327 US20250018697A1 (en) 2022-03-25 2024-09-18 Laminate and manufacturing method of laminate

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022050807 2022-03-25
JP2022-050807 2022-03-25

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US18/889,327 Continuation US20250018697A1 (en) 2022-03-25 2024-09-18 Laminate and manufacturing method of laminate

Publications (1)

Publication Number Publication Date
WO2023181489A1 true WO2023181489A1 (ja) 2023-09-28

Family

ID=88100383

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/042287 Ceased WO2023181489A1 (ja) 2022-03-25 2022-11-14 積層体及び積層体の製造方法

Country Status (6)

Country Link
US (1) US20250018697A1 (cg-RX-API-DMAC7.html)
EP (1) EP4501621A4 (cg-RX-API-DMAC7.html)
JP (1) JPWO2023181489A1 (cg-RX-API-DMAC7.html)
KR (1) KR20240151785A (cg-RX-API-DMAC7.html)
CN (1) CN118900765A (cg-RX-API-DMAC7.html)
WO (1) WO2023181489A1 (cg-RX-API-DMAC7.html)

Citations (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013208753A (ja) * 2012-03-30 2013-10-10 Fujifilm Corp 機能性フィルムおよび機能性フィルムの製造方法
JP2015182274A (ja) * 2014-03-24 2015-10-22 富士フイルム株式会社 ガスバリアフィルムおよびガスバリアフィルムの製造方法
JP2015193214A (ja) * 2014-01-08 2015-11-05 キヤノン電子株式会社 繊維強化積層体、シャッタ羽根及びシャッタ装置並びにカメラ
WO2015190572A1 (ja) * 2014-06-13 2015-12-17 Jnc株式会社 ガスバリアフィルム積層体とそれを用いた電子部品
JP2017159586A (ja) * 2016-03-10 2017-09-14 富士フイルム株式会社 ガスバリアフィルム
WO2018181572A1 (ja) * 2017-03-29 2018-10-04 帝人株式会社 ハードコート層付高分子基板
WO2019065020A1 (ja) * 2017-09-27 2019-04-04 富士フイルム株式会社 ガスバリアフィルム
JP2019119086A (ja) 2017-12-28 2019-07-22 ランテクニカルサービス株式会社 基板の接合方法、透明基板積層体及び基板積層体を備えるデバイス
US20190229281A1 (en) * 2017-11-15 2019-07-25 Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd. Flexible substrate and fabricating method thereof
JP2022050807A (ja) 2020-09-18 2022-03-31 株式会社日本製鋼所 積層成形システム

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6420032B1 (en) * 1999-03-17 2002-07-16 General Electric Company Adhesion layer for metal oxide UV filters
WO2018211850A1 (ja) * 2017-05-19 2018-11-22 富士フイルム株式会社 ガスバリアフィルムおよびガスバリアフィルムの製造方法
CN109994688B (zh) * 2017-12-29 2021-09-17 宁德时代新能源科技股份有限公司 复合隔离膜及其制备方法、使用其的电化学装置
JPWO2019187981A1 (ja) * 2018-03-28 2021-02-25 富士フイルム株式会社 ガスバリアフィルム

Patent Citations (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2013208753A (ja) * 2012-03-30 2013-10-10 Fujifilm Corp 機能性フィルムおよび機能性フィルムの製造方法
JP2015193214A (ja) * 2014-01-08 2015-11-05 キヤノン電子株式会社 繊維強化積層体、シャッタ羽根及びシャッタ装置並びにカメラ
JP2015182274A (ja) * 2014-03-24 2015-10-22 富士フイルム株式会社 ガスバリアフィルムおよびガスバリアフィルムの製造方法
WO2015190572A1 (ja) * 2014-06-13 2015-12-17 Jnc株式会社 ガスバリアフィルム積層体とそれを用いた電子部品
JP2017159586A (ja) * 2016-03-10 2017-09-14 富士フイルム株式会社 ガスバリアフィルム
WO2018181572A1 (ja) * 2017-03-29 2018-10-04 帝人株式会社 ハードコート層付高分子基板
WO2019065020A1 (ja) * 2017-09-27 2019-04-04 富士フイルム株式会社 ガスバリアフィルム
US20190229281A1 (en) * 2017-11-15 2019-07-25 Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd. Flexible substrate and fabricating method thereof
JP2019119086A (ja) 2017-12-28 2019-07-22 ランテクニカルサービス株式会社 基板の接合方法、透明基板積層体及び基板積層体を備えるデバイス
JP2022050807A (ja) 2020-09-18 2022-03-31 株式会社日本製鋼所 積層成形システム

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4501621A4

Also Published As

Publication number Publication date
EP4501621A1 (en) 2025-02-05
KR20240151785A (ko) 2024-10-18
CN118900765A (zh) 2024-11-05
EP4501621A4 (en) 2025-07-16
JPWO2023181489A1 (cg-RX-API-DMAC7.html) 2023-09-28
US20250018697A1 (en) 2025-01-16

Similar Documents

Publication Publication Date Title
JP6527053B2 (ja) ガスバリアフィルムおよびガスバリアフィルムの転写方法
JP6305319B2 (ja) 波長変換部材及びそれを備えたバックライトユニット、液晶表示装置並びに波長変換部材の製造方法
JP5730235B2 (ja) ガスバリアフィルムおよびガスバリアフィルムの製造方法
EP2228463B1 (en) Method for manufacturing a functional film
JP6524702B2 (ja) ガスバリア性フィルムの製造方法及びガスバリア性フィルム
WO2016056605A1 (ja) 積層体の製造方法
JPWO2010026869A1 (ja) 複合フィルム、ガスバリアフィルム及びその製造方法並びに有機エレクトロルミネッセンス素子
JPWO2010024149A1 (ja) 複合フィルム、ガスバリアフィルム及びその製造方法並びに有機エレクトロルミネッセンス素子
JP6475842B2 (ja) 機能性フィルムの製造方法及び製造装置
JP5318020B2 (ja) 機能性フィルムの製造方法
JP4282360B2 (ja) ガスバリア性プラスチックフィルム
JP5198493B2 (ja) 機能性フィルムの製造方法
US20250018697A1 (en) Laminate and manufacturing method of laminate
JP5364001B2 (ja) 機能性フィルムの製造方法
WO2010026852A1 (ja) 樹脂フィルム及びその製造方法並びに有機エレクトロルミネッセンス素子
JP5331740B2 (ja) 機能性フィルム
JP6998734B2 (ja) 積層体及びこれを含むデバイス
JP5874975B2 (ja) ガスバリア性フィルム
JP6317681B2 (ja) 機能性フィルムおよび機能性フィルムの製造方法
JP2004349112A (ja) 透明導電性フィルム及び透明導電性シートの製造方法、及びタッチパネル
JP6409258B2 (ja) ガスバリアフィルム積層体とそれを用いた電子部品
US20250269636A1 (en) Method of manufacturing gas barrier film packaging material
JPWO2015053189A1 (ja) ガスバリアーフィルム及びその製造方法
JP2010069693A (ja) 積層体及びその製造装置
JPWO2017086034A1 (ja) ガスバリアー性フィルム、照明装置及び表示装置

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22933619

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2024509737

Country of ref document: JP

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 20247030376

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020247030376

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 202280093717.8

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 2022933619

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2022933619

Country of ref document: EP

Effective date: 20241025