WO2021200967A1 - 複合体、及び放熱部材 - Google Patents

複合体、及び放熱部材 Download PDF

Info

Publication number
WO2021200967A1
WO2021200967A1 PCT/JP2021/013572 JP2021013572W WO2021200967A1 WO 2021200967 A1 WO2021200967 A1 WO 2021200967A1 JP 2021013572 W JP2021013572 W JP 2021013572W WO 2021200967 A1 WO2021200967 A1 WO 2021200967A1
Authority
WO
WIPO (PCT)
Prior art keywords
sintered body
nitride sintered
boron nitride
complex
composite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2021/013572
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
紗緒梨 井之上
翔二 岩切
賢久 上島
亮 吉松
竜士 古賀
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Denka Co Ltd
Original Assignee
Denka Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Denka Co Ltd filed Critical Denka Co Ltd
Priority to JP2022512550A priority Critical patent/JPWO2021200967A1/ja
Publication of WO2021200967A1 publication Critical patent/WO2021200967A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C04—CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
    • C04B—LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
    • C04B35/00—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products
    • C04B35/515—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics
    • C04B35/58—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides
    • C04B35/583—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides based on boron nitride
    • C—CHEMISTRY; METALLURGY
    • C04—CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
    • C04B—LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
    • C04B41/00—After-treatment of mortars, concrete, artificial stone or ceramics; Treatment of natural stone
    • C04B41/80—After-treatment of mortars, concrete, artificial stone or ceramics; Treatment of natural stone of only ceramics
    • C04B41/81—Coating or impregnation
    • C04B41/82—Coating or impregnation with organic materials
    • C04B41/83—Macromolecular compounds
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W40/00—Arrangements for thermal protection or thermal control
    • H10W40/20—Arrangements for cooling
    • H10W40/25—Arrangements for cooling characterised by their materials

Definitions

  • This disclosure relates to a complex and a heat radiating member.
  • thermal interface materials that have electrical insulation properties for electronic components or printed wiring boards. It has been used to attach it to a heat sink.
  • a composite heat dissipation member composed of a resin and ceramics such as boron nitride is used.
  • Patent Document 1 proposes a technique for reducing the anisotropy of thermal conductivity while having excellent thermal conductivity by setting the degree of orientation and the graphitization index within a predetermined range.
  • the present disclosure provides a complex having excellent adhesiveness to other members. Further, in the present disclosure, by providing the above-mentioned composite, a heat radiating member having sufficiently high reliability is provided.
  • the present disclosure is a composite containing a nitride sintered body having a porous structure and a semi-cured product of a thermosetting resin composition impregnated in the nitride sintered body, and is applied in the thickness direction at 5 MPa.
  • a composite having a thickness change rate of 2% or more when pressed. Such a complex is deformed at a predetermined thickness change rate when, for example, it is sandwiched between a pair of opposing members and pressurized.
  • the composite has a nitride sintered body having a porous structure, and the nitride sintered body is impregnated with a semi-cured product of a thermosetting resin composition.
  • the complex When this complex is sandwiched between a pair of opposing members and pressed to join, the complex is deformed at a predetermined rate of change in thickness. When deformed, the resin component contained in the complex exudes. By the action of the exuded resin component, the complex can be firmly adhered to other members. Therefore, it has excellent adhesiveness.
  • the thickness change rate of the complex may be 35% or less. By having such a thickness change rate, the shape can be maintained to some extent even if pressure is applied when adhering to other members. Therefore, for example, the dimensional accuracy of the electronic component can be improved.
  • the porosity of the boron nitride sintered body contained in the above complex may be 40 to 75% by volume. Thereby, the impregnation amount of the semi-cured product of the thermosetting resin composition can be sufficiently increased while maintaining the strength and thermal conductivity of the boron nitride sintered body. Such a complex can achieve both excellent insulation and adhesiveness at a high level.
  • the porosity is the total volume ratio of the pores filled with the resin and the pores not filled with the resin.
  • the bulk density of the boron nitride sintered body contained in the complex may be 600 to 1400 kg / m 3 .
  • the impregnation amount of the semi-cured product of the thermosetting resin composition can be sufficiently increased while maintaining the strength and thermal conductivity of the boron nitride sintered body.
  • Such a complex can achieve both excellent insulation and adhesiveness at a high level.
  • the orientation index of the boron nitride sintered body contained in the above complex may be 20 or less. Thereby, the anisotropy of thermal conductivity can be sufficiently reduced.
  • the present disclosure provides a heat radiating member having the above-mentioned complex in one aspect. Since this heat radiating member has the above-mentioned composite, it has excellent adhesiveness.
  • FIG. 1 is a perspective view of a complex in one embodiment.
  • the sheet-like composite 10 contains a nitride sintered body 20 having a porous structure and a semi-cured product of a thermosetting resin composition impregnated in the nitride sintered body 20.
  • the nitride sintered body 20 contains boron nitride particles and pores formed by sintering primary boron nitride particles.
  • the thickness change rate when pressurized at 5 MPa in the thickness direction may be 2% or more, or 5% or more.
  • the thickness change rate may be 35% or less, or 20% or less.
  • An example of the thickness change rate is 2 to 35%.
  • the thickness change rate can be measured at a measurement temperature of 200 ° C. using a precision universal testing machine (trade name: Autograph AG-X) manufactured by Shimadzu Corporation. If the main surfaces 10a and 10b of the complex 10 have irregularities or protrusions that affect the measurement of the thickness change rate, the main surfaces 10a and 10b are processed to remove the irregularities. These processes may be performed using, for example, a machining center (trade name: Dualvertical 635 eco) operated by MORI SEIKI.
  • the thickness t of the complex 10 may be less than 2 mm, less than 1 mm, and less than 0.5 mm. From the viewpoint of maintaining a certain level of strength, the thickness t of the complex 10 may be 0.1 mm or more, or 0.2 mm or more. An example of the thickness of the complex 10 is 0.1 mm or more and less than 2 mm.
  • the areas of the main surfaces 10a and 10b of the complex 10 may be 25 mm 2 or more, 100 mm 2 or more, 500 mm 2 or more, 800 mm 2 or more, 1000 mm 2 or more, respectively. May be.
  • the thickness t of the nitride sintered body 20 may be less than 2 mm, less than 1 mm, or less than 0.5 mm. From the viewpoint of ease of molding, the thickness of the nitride sintered body 20 may be 0.1 mm or more, or 0.2 mm or more.
  • the main surface 20a of the nitride sintered body 20, the area of the 20b, may be at 25 mm 2 or more, may be at 100 mm 2 or more, may be at 500 mm 2 or more, may be at 800 mm 2 or more, 1000 mm 2 It may be the above.
  • the average pore diameter of the pores contained in the nitride sintered body 20 may be less than 10 ⁇ m.
  • the average pore size of the pores is determined based on the pore size distribution when pressure is applied while increasing the pressure from 0.5 psia to 60,000 psia using a mercury porosimeter.
  • the horizontal axis is the pore diameter and the vertical axis is the cumulative pore volume
  • the pore diameter when the cumulative pore volume reaches 50% of the total pore volume is the average pore diameter.
  • the mercury porosimeter one manufactured by Shimadzu Corporation can be used.
  • the porosity of the nitride sintered body 20, that is, the volume ratio of the pores in the nitride sintered body 20 may be 40 to 75% by volume or 45 to 70% by volume. If the porosity becomes too large, the strength and thermal conductivity of the nitride sintered body tend to decrease. On the other hand, if the porosity becomes too small, the content of the semi-cured product of the thermosetting resin composition when the composite is produced tends to decrease.
  • the bulk density [B (kg / m 3 )] was calculated from the volume and mass of the nitride sintered body 20, and the bulk density and the theoretical density of boron nitride [2280 (kg / m 3 )] were used. Therefore, it can be obtained by the following formula (2).
  • Porosity (% by volume) [1- (B / 2280)] x 100 (2)
  • the bulk density B may be 600 to 1400 kg / m 3 or 800 to 1200 kg / m 3 . If the bulk density B becomes too small, the strength of the nitride sintered body 20 tends to decrease. On the other hand, if the bulk density B becomes too large, the impregnation amount of the semi-cured product of the thermosetting resin composition tends to decrease, and the insulating property of the composite tends to decrease.
  • the thermal conductivity of the nitride sintered body 20 may be 10 W / (m ⁇ K) or more, 15 W / (m ⁇ K) or more, and 20 W / (m ⁇ K) or more. , 25 W / (m ⁇ K) or more.
  • the thermal conductivity (H) can be calculated by the following formula (3).
  • the thermal conductivity (H) may be 70 W / (m ⁇ K) or less, 60 W / (m ⁇ K) or less, and 50 W / (m ⁇ K) or less.
  • H A ⁇ B ⁇ C (3)
  • H is the thermal conductivity (W / (m ⁇ K))
  • A is the thermal diffusivity (m 2 / sec)
  • B is the bulk density (kg / m 3 )
  • C is the specific heat capacity. (J / (kg ⁇ K)) is shown.
  • the thermal diffusivity A can be measured by a laser flash method.
  • the bulk density B can be obtained from the volume and mass of the nitride sintered body 20.
  • the specific heat capacity C can be measured using a differential scanning calorimeter.
  • the nitride sintered body 20 may be a boron nitride sintered body.
  • the boron nitride sintered body may contain components other than boron nitride.
  • the content of boron nitride in the boron nitride sintered body may be 90% by mass or more, 95% by mass or more, and 98% by mass or more.
  • the nitride sintered body 20 has a sheet shape (thin plate shape). Since the sheet-shaped nitride sintered body 20 has a small thickness t 0 , the resin composition can be smoothly impregnated. As a result, the pores of the nitride sintered body are sufficiently filled with the semi-cured product, and a composite having excellent insulating properties can be obtained.
  • the orientation index of the boron nitride crystal in the boron nitride sintered body may be 20 or less, 18 or less, and 15 or less. Thereby, the anisotropy of thermal conductivity can be sufficiently reduced. Therefore, in the case of a sheet like a boron nitride sintered body, the thermal conductivity along the thickness direction can be sufficiently increased.
  • the thermal conductivity (H) along the thickness direction of the boron nitride sintered body is preferably the above-mentioned value.
  • the orientation index of the boron nitride sintered body may be 0.5 or more, 3 or more, or 5 or more.
  • the orientation index in the present disclosure is an index for quantifying the degree of orientation of boron nitride crystals.
  • the orientation index can be calculated by the peak intensity ratio [I (002) / I (100)] of the (002) plane and the (100) plane of boron nitride measured by an X-ray diffractometer.
  • the shape of the nitride sintered body is not limited to the shape shown in FIG. 1, and may be, for example, a disk-shaped sheet or a C-shaped sheet in which the main surfaces 20a and 20b are curved.
  • the thickness change rate can be measured by processing into a sheet as shown in FIG.
  • the block-shaped nitride sintered body may be cut and / or polished to be processed into a sheet shape as shown in FIG.
  • material loss will occur. Therefore, if a sheet-shaped nitride sintered body is produced using the sheet-shaped molded body, material loss can be reduced. Thereby, the yield of the nitride sintered body and the composite can be improved.
  • the block-shaped nitride sintered body is a polyhedron, for example, all sides have a suitable length, and the block-shaped nitride sintered body has a larger thickness than the sheet-shaped nitride sintered body. That is, the block shape means a shape that can be divided into a plurality of sheet shapes (thin plate shapes) by cutting.
  • the composite according to one embodiment is a composite of a nitride sintered body and a semi-cured product of a thermosetting resin composition, and is at least a part of the pores of the above-mentioned nitride sintered body and the nitride sintered body. It has a semi-cured product of a thermosetting resin composition filled in.
  • the thermosetting resin composition include epoxy resin, silicone resin, cyanate resin, silicone rubber, acrylic resin, phenol resin, melamine resin, urea resin, bismaleimide resin unsaturated polyester, fluororesin, polyimide, polyamideimide, and the like.
  • the thermosetting resin composition may contain an epoxy resin from the viewpoint of improving heat resistance and adhesive strength to the circuit.
  • the resin may contain a silicone resin from the viewpoint of improving heat resistance, flexibility, and adhesion to a heat sink or the like.
  • the semi-cured product of the thermosetting resin composition is also referred to as a B stage state.
  • the content of the boron nitride particles in the complex may be 25 to 65% by volume or 39 to 48% by volume based on the total volume of the complex.
  • the content of the semi-cured product of the thermosetting resin composition in the complex may be 35 to 75% by volume or 52 to 61% by volume based on the total volume of the complex.
  • a composite containing boron nitride particles and a semi-cured product of a thermosetting resin composition at such a ratio can achieve both high adhesiveness and high thermal conductivity at a high level.
  • the content of the resin containing the semi-cured product in the complex may be 10 to 70% by mass, 10 to 60% by mass, or 20 to 60% by mass based on the total mass of the complex. It may be 20 to 55% by mass, and may be 25 to 55% by mass.
  • a complex containing a resin in such a ratio can achieve both high adhesiveness and thermal conductivity at a high level.
  • the content of the resin in the complex can be determined by heating the complex to decompose and remove the resin, and calculating the mass of the resin from the mass difference before and after heating.
  • the filling rate of the resin containing the semi-cured product in the complex may be 80% by volume or more, 90% by volume or more, or 92% by volume or more.
  • the resin filling rate is the volume ratio of the pores filled with the resin (semi-cured product + cured product) among all the pores in the boron nitride sintered body.
  • the porosity in the complex may be 20% by volume or less, 10% by volume or less, 8% by volume or less, 6% by volume or less, and 5% by volume or less. It may be 4% by volume or less. As a result, both high adhesiveness and high insulation can be achieved at a sufficiently high level.
  • the complex may further contain other components in addition to the nitride sintered body and the semi-cured product of the thermosetting resin composition filled in the pores thereof.
  • other components include a curing agent, an inorganic filler, a silane coupling agent, a defoaming agent, a surface conditioner, a wet dispersant and the like.
  • the inorganic filler may contain one or more selected from the group consisting of aluminum oxide, silicon oxide, zinc oxide, silicon nitride, aluminum nitride and aluminum hydroxide. Thereby, the thermal conductivity of the complex can be further improved.
  • the semi-cured product may contain a completely cured product (C stage). The cured product and the semi-cured product may be collectively referred to as a resin.
  • the composite may be in the form of a sheet (thin plate shape) as shown in FIG. 1, similarly to the nitride sintered body. Since the sheet-shaped complex 10 has a small thickness, it can be suitably used as a heat radiating member for electronic devices and the like. Moreover, the resin composition is sufficiently impregnated.
  • the composite 10 contains the above-mentioned nitride sintered body and a semi-cured product of a thermosetting resin composition.
  • the complex 10 is sandwiched between a pair of opposing members and pressed to join, the complex 10 is deformed at a predetermined thickness change rate.
  • the resin component impregnated in the complex exudes.
  • the complex 10 can be firmly adhered to other members by the action of the exuded resin component. Therefore, the complex 10 is excellent in adhesiveness to other members. Therefore, the complex 10 has sufficiently high reliability.
  • Such a complex 10 can be suitably used as a heat radiating member.
  • the shape of the heat radiating member may be the same as that of the complex 10 shown in FIG. 1, or may be different.
  • the production method of this example includes a sintering step of sintering boron nitride powder to obtain a block-shaped boron nitride sintered body.
  • the raw material powder include amorphous boron nitride powder having an average particle size of 0.5 to 10 ⁇ m and hexagonal boron nitride powder having an average particle size of 3.0 to 40 ⁇ m. These powders may be mixed using a Henschel mixer or the like, or may be mixed in a slurry form in water or an ethanol solution using a disparizer.
  • a slurry containing such boron nitride powder may be spheroidized by a spray dryer or the like, molded, and then sintered to obtain a boron nitride sintered body.
  • a mold may be used for molding, or a cold isotropic pressing (CIP) method may be used.
  • the average particle size of each of the above-mentioned boron nitride powders is a particle size of 50% of the cumulative value of the cumulative particle size distribution in the particle size distribution measurement by the laser diffraction light scattering method.
  • the particle size distribution measuring machine include "MT3300EX" (manufactured by Nikkiso Co., Ltd.).
  • water is used as a solvent
  • hexametaphosphate is used as a dispersant
  • a homogenizer is used for 30 seconds to carry out a dispersion treatment with an output of 20 W.
  • 1.33 is used for the refractive index of water
  • 1.80 is used for the refractive index of the boron nitride powder.
  • the measurement time per measurement is 30 seconds.
  • a sintering aid When sintering the boron nitride powder, a sintering aid may be used.
  • the sintering aid may be, for example, an oxide of a rare earth element such as itria oxide, alumina oxide and magnesium oxide, a carbonate of an alkali metal such as lithium carbonate and sodium carbonate, and boric acid.
  • the amount of the sintering aid added may be, for example, 1.5 to 25 parts by mass with respect to 100 parts by mass of the total of the boron nitride powder and the sintering aid. , 3.0 to 22 parts by mass.
  • the sintering temperature in the sintering step may be, for example, 1600 ° C. or higher, or 1700 ° C. or higher.
  • the sintering temperature may be, for example, 2200 ° C. or lower, 2100 ° C. or lower, or 2000 ° C. or lower.
  • the sintering time may be, for example, 1 hour or more, or 30 hours or less.
  • the atmosphere at the time of sintering may be, for example, an atmosphere of an inert gas such as nitrogen, helium, and argon.
  • a batch type furnace, a continuous type furnace, or the like can be used.
  • the batch type furnace include a high frequency furnace, a muffle furnace, a tube furnace, an atmosphere furnace, and the like.
  • the continuous furnace include a rotary kiln, a screw conveyor furnace, a tunnel furnace, a belt furnace, a pusher furnace, a koto-shaped continuous furnace, and the like. In this way, a block-shaped boron nitride sintered body can be obtained.
  • the method for producing the complex of this example includes an impregnation step and a cutting step of impregnating a block-shaped (for example, a bulk body having a thickness of more than 2 mm) boron nitride sintered body with a resin composition.
  • the thermosetting resin composition may contain a main agent, a curing agent and a solvent from the viewpoint of improving fluidity and handleability.
  • an inorganic filler, a silane coupling agent, a defoaming agent, a surface conditioner, a wet dispersant and the like may be contained.
  • thermosetting resin composition one that becomes the semi-cured product mentioned in the above description of the complex by the semi-curing reaction can be used.
  • solvent include aliphatic alcohols such as ethanol and isopropanol, 2-methoxyethanol, 1-methoxyethanol, 2-ethoxyethanol, 1-ethoxy-2-propanol, 2-butoxyethanol and 2- (2-methoxyethoxy).
  • Ether alcohols such as ethanol, 2- (2-ethoxyethoxy) ethanol, 2- (2-butoxyethoxy) ethanol, glycol ethers such as ethylene glycol monomethyl ether and ethylene glycol monobutyl ether, acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl
  • ketones such as ketones and hydrocarbons such as toluene and xylene. One of these may be contained alone, or two or more thereof may be contained in combination.
  • Impregnation is performed by adhering a thermosetting resin composition to a boron nitride sintered body.
  • the boron nitride sintered body may be immersed in a thermosetting resin composition. It may be carried out under atmospheric pressure, pressurization, or depressurization conditions in the immersed state.
  • a thermosetting resin composition can be applied to the boron nitride sintered body to impregnate it. In this way, the pores of the boron nitride sintered body can be filled with the resin.
  • the impregnation step may be performed in an impregnation device provided with a closed container.
  • the pressure in the impregnating device may be increased to be higher than the atmospheric pressure and impregnated under pressurized conditions.
  • the depressurization condition and the pressurization condition may be repeated a plurality of times.
  • the impregnation step may be performed while heating.
  • thermosetting resin composition impregnated in the pores of the boron nitride sintered body becomes a semi-cured product after semi-curing proceeds or the solvent volatilizes.
  • a composite having a boron nitride sintered body and a semi-cured product filled in its pores is obtained. It is not necessary that all the pores are filled with the semi-cured product, and some of the pores may not be filled with the semi-cured product.
  • Boron nitride sintered bodies and complexes may contain both closed and open pores.
  • the impregnation step there may be a curing step of curing the thermosetting resin composition filled in the pores.
  • the curing step for example, the composite filled with the thermosetting resin is taken out from the impregnation device, heated and / or irradiated with light depending on the type of the resin composition (or the curing agent added as needed). Semi-cures the resin.
  • the impregnation step may be performed by combining impregnation under reduced pressure conditions and impregnation under pressurized conditions.
  • the pressure in the impregnation device when the impregnation step is carried out under reduced pressure conditions may be, for example, 1000 Pa or less, 500 Pa or less, 100 Pa or less, 50 Pa or less, or 30 Pa or less.
  • the pressure in the impregnation device may be, for example, 1 MPa or more, 3 MPa or more, 10 MPa or more, or 30 MPa or more.
  • the solution containing the thermosetting resin composition may be heated.
  • the viscosity of the solution can be adjusted and the impregnation of the thermosetting resin composition can be promoted.
  • the viscosity of the solution containing the thermosetting resin composition at the time of impregnation may be, for example, 500 mPa ⁇ s or less.
  • the thermosetting resin composition can be sufficiently impregnated into the boron nitride sintered body.
  • the nitride sintered body is kept immersed in a solution containing a thermosetting resin composition for a predetermined time.
  • the predetermined time may be, for example, 5 hours or more, or 10 hours or more.
  • thermosetting resin composition filled in the pores.
  • the curing step for example, the composite filled with the thermosetting resin composition is taken out from the impregnation device and heated according to the type of the thermosetting resin composition (or the curing agent added as needed). And / or light irradiation causes the thermosetting resin composition to be semi-cured.
  • "Semi-hardening" also referred to as B stage
  • B stage means that it can be further hardened by a subsequent hardening treatment. Utilizing the fact that it is in a semi-cured state, it may be temporarily pressure-bonded to an adherend such as a metal substrate and then heated to adhere to the adherend.
  • thermosetting resin composition By further curing the semi-cured product, it can be in a "completely cured" (also referred to as C stage) state. Whether or not the thermosetting resin composition is in a semi-cured state can be confirmed by, for example, a differential scanning calorimeter.
  • the obtained resin impregnated body is cut using, for example, a wire saw.
  • the wire saw may be, for example, a multi-cut wire saw or the like. ) Can be cut and prepared. In this way, a sheet-like complex can be obtained.
  • Nitride sintered bodies other than the boron nitride sintered body can be produced by a known method.
  • a boron nitride sintered body may be obtained by hot pressing in which molding and sintering are performed at the same time.
  • Example 1 ⁇ Preparation of Boron Nitride Sintered Body> Hexagonal boron nitride powder (oxygen content 0.8% by mass, boron nitride purity 99.0% by mass) having an average particle size of 8.0 ⁇ m is 40.0% by mass, and the average particle size is 13.0 ⁇ m. A certain hexagonal boron nitride powder (oxygen content: 0.3% by mass, boron nitride purity: 99.0% by mass) is measured so as to be 60.0% by mass, and these are mixed to prepare a raw material powder. bottom.
  • a sintering aid was prepared by blending powdered boric acid and calcium carbonate. In the preparation, 60 parts by mass of calcium carbonate was added to 100 parts by mass of boric acid. 14 parts by mass of a sintering aid and 10 parts by mass of a binder (polyvinyl alcohol (“Gosenol”, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.)) were blended with respect to 100 parts by mass of the raw material powder. The obtained compound was heated and stirred at 50 ° C. until it was dissolved, and then spheroidized at a drying temperature of 230 ° C. using a spray dryer. In this way, a spheroidized mixed powder was prepared. A rotary atomizer was used as the spheroidizing device of the spray dryer.
  • the above mixed powder was filled in a cold isotropic pressure (CIP) device (manufactured by Kobe Steel, Ltd., trade name: ADW800) and compressed at a pressure of 30 MPa to prepare a molded product.
  • CIP cold isotropic pressure
  • the produced molded product was sintered by holding it at 2000 ° C. for 10 hours using a batch type high frequency furnace (manufactured by Fuji Dempa Kogyo Co., Ltd., trade name: FTH-300-1H).
  • FTH-300-1H a batch type high frequency furnace
  • the firing was carried out by adjusting the inside of the furnace under a nitrogen atmosphere while flowing nitrogen into the furnace in a standard state so that the flow rate was 10 L / min.
  • H is the thermal conductivity (W / (m ⁇ K))
  • A is the thermal diffusivity (m 2 / sec)
  • B is the bulk density (kg / m 3 )
  • C is the specific heat capacity. (J / (kg ⁇ K)) is shown.
  • a xenon flash analyzer manufactured by NETZSCH, trade name: LFA447NanoFlash was used as the measuring device.
  • the bulk density B was calculated from the volume and mass of the boron nitride sintered body.
  • the specific heat capacity C was measured using a differential scanning calorimeter (manufactured by Rigaku Co., Ltd., device name: ThermoPlusEvo DSC8230).
  • the results of thermal conductivity H and bulk density B are shown in Table 1.
  • the orientation index [I (002) / I (100)] of the boron nitride sintered body was determined using an X-ray diffractometer (manufactured by Rigaku Co., Ltd., trade name: ULTIMA-IV).
  • the measurement sample (boron nitride sintered body) set in the sample holder of the X-ray diffractometer was irradiated with X-rays to perform baseline correction. Then, the peak intensity ratio of the (002) plane and the (100) plane of boron nitride was calculated. This was defined as the orientation index [I (002) / I (100)].
  • the results are as shown in Table 1.
  • Epoxy resin manufactured by Mitsubishi Chemical Co., Ltd., trade name: Epicoat 807
  • curing agent manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name: Acmex H-84B
  • the boron nitride sintered body was immersed in the thermosetting resin composition containing the above, and the boron nitride sintered body was impregnated with the thermosetting resin composition. After impregnation, the thermosetting resin composition was semi-cured by heating at a temperature of 150 ° C.
  • Resin filling rate in the composite ((composite bulk density-boron nitride sintered bulk density) / (complex theoretical density-boron nitride sintered bulk density)) x 100. ⁇ ⁇ (6)
  • Theoretical density of composite true density of boron nitride sintered body + true density of resin x (1-bulk density of boron nitride sintered body / true density of boron nitride sintered body) ... (7)
  • the bulk density of the boron nitride sintered body conforms to the measurement method of density and specific gravity by geometric measurement of JIS Z 8807: 2012, and is a sheet-shaped (rectangular) boron nitride sintered body (composite). It was obtained from the volume calculated from the length of each side (measured by a caliper) and the mass measured by an electronic balance (see item 9 of JIS Z 8807: 2012).
  • the true density of the boron nitride sintered body and the resin conforms to the method of measuring the density and specific gravity by the gas substitution method of JIS Z 8807: 2012, and the volume of the boron nitride sintered body and the resin measured using a dry automatic densitometer. (Refer to equations (14) to (17) in paragraph 11 of JIS Z 8807: 2012).
  • the resin content in the complex sheet is as shown in Table 2.
  • the content (% by mass) of this resin is the mass ratio of the semi-cured product to the entire complex.
  • the content of the semi-cured product was calculated by calculating the mass of the semi-cured product from the mass difference between the boron nitride sintered body and the composite, and dividing the mass of the semi-cured product by the mass of the composite.
  • the cohesive fracture portion is the area of the portion of the adhesive surface of the composite that has been adhered to the copper foil and that the composite has broken.
  • Example 2 Boron nitride firing was performed in the same procedure as in Example 1 except that when the molded product was produced, the mixed powder was compressed at a pressure of 35 MPa with a cold isotropic pressure (CIP) device to obtain the molded product. Bounds and complexes were made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 3 Boron nitride sintered body and composite were obtained by the same procedure as in Example 1 except that the molded product was obtained by compressing it with a cold isotropic pressure (CIP) device at a pressure of 90 MPa when producing the molded product. The body was made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 4 Boron nitride sintered body and composite were obtained by the same procedure as in Example 1 except that the molded product was obtained by compressing it with a cold isotropic pressure (CIP) device at a pressure of 10 MPa when producing the molded product. The body was made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 5 Amorphous boron nitride powder (oxygen content: 1.8% by mass, boron nitride purity: 97.2% by mass) having an average particle size of 0.8 ⁇ m is 40.0% by mass, and an average particle size is 13.0 ⁇ m.
  • Hexagonal boron nitride powder (oxygen content: 0.3% by mass, boron nitride purity: 99.0% by mass) was measured so as to be 60.0% by mass, and blended to prepare a raw material powder. ..
  • a boron nitride sintered body and a complex were prepared in the same procedure as in Example 1 except that this raw material powder was used. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 6 The boron nitride sintered body and the composite were prepared in the same procedure as in Example 1 except that the method for producing the molded product was changed from cold isotropic pressure (CIP) to mold molding (molding pressure: 50 MPa). Made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 7 The boron nitride sintered body and the composite were prepared in the same procedure as in Example 1 except that the method for producing the molded product was changed from cold isotropic pressure (CIP) to mold molding (molding pressure: 15 MPa). Made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 8 No spheroidizing treatment was performed with a spray dryer, and a mixed powder was prepared by stirring the raw material powder and the sintering aid using a Henschel mixer, which was used in a cold isotropic pressurizer.
  • a boron nitride sintered body and a composite were prepared in the same procedure as in Example 1 except that the molded product was produced.
  • Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 9 A boron nitride sintered body and a composite were prepared in the same procedure as in Example 8 except that the molded product was produced by mold molding (molding pressure: 30 MPa) instead of the cold isotropic pressurizing device. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Hexagonal boron nitride powder (oxygen content: 0.3% by mass, boron nitride purity: 99.1% by mass) having an average particle size of 18.0 ⁇ m is 40.0% by mass, and the average particle size is 13.
  • Hexagonal boron nitride powder (oxygen content: 0.3% by mass, boron nitride purity: 99.0% by mass), which is 0 ⁇ m, is measured so as to be 60.0% by mass, and these are mixed and used as a raw material.
  • a powder was prepared.
  • a boron nitride sintered body and a complex were prepared in the same procedure as in Example 1 except that this raw material powder was used.
  • Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.
  • Example 2 Boron nitride sintered body and composite were obtained by the same procedure as in Example 1 except that the molded product was obtained by compressing it with a cold isotropic pressure (CIP) device at a pressure of 150 MPa when producing the molded product. The body was made. Each measurement of the boron nitride sintered body and the composite was carried out in the same manner as in Example 1. The results are as shown in Tables 1 and 2.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Ceramic Engineering (AREA)
  • Materials Engineering (AREA)
  • Structural Engineering (AREA)
  • Organic Chemistry (AREA)
  • Manufacturing & Machinery (AREA)
  • Cooling Or The Like Of Semiconductors Or Solid State Devices (AREA)
  • Ceramic Products (AREA)
PCT/JP2021/013572 2020-03-31 2021-03-30 複合体、及び放熱部材 Ceased WO2021200967A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2022512550A JPWO2021200967A1 (cg-RX-API-DMAC7.html) 2020-03-31 2021-03-30

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2020064251 2020-03-31
JP2020-064251 2020-03-31

Publications (1)

Publication Number Publication Date
WO2021200967A1 true WO2021200967A1 (ja) 2021-10-07

Family

ID=77927205

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2021/013572 Ceased WO2021200967A1 (ja) 2020-03-31 2021-03-30 複合体、及び放熱部材

Country Status (2)

Country Link
JP (1) JPWO2021200967A1 (cg-RX-API-DMAC7.html)
WO (1) WO2021200967A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2023190559A1 (ja) * 2022-03-30 2023-10-05 デンカ株式会社 放熱構造体

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2014196496A1 (ja) * 2013-06-03 2014-12-11 電気化学工業株式会社 樹脂含浸窒化ホウ素焼結体およびその用途
US20180148623A1 (en) * 2016-11-28 2018-05-31 Infineon Technologies Ag Resin-Impregnated Boron Nitride Body and a Method for Producing a Resin-Impregnated Boron Nitride Body
WO2018181606A1 (ja) * 2017-03-29 2018-10-04 デンカ株式会社 伝熱部材及びこれを含む放熱構造体
WO2019111978A1 (ja) * 2017-12-05 2019-06-13 デンカ株式会社 窒化物系セラミックス樹脂複合体

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2014196496A1 (ja) * 2013-06-03 2014-12-11 電気化学工業株式会社 樹脂含浸窒化ホウ素焼結体およびその用途
US20180148623A1 (en) * 2016-11-28 2018-05-31 Infineon Technologies Ag Resin-Impregnated Boron Nitride Body and a Method for Producing a Resin-Impregnated Boron Nitride Body
WO2018181606A1 (ja) * 2017-03-29 2018-10-04 デンカ株式会社 伝熱部材及びこれを含む放熱構造体
WO2019111978A1 (ja) * 2017-12-05 2019-06-13 デンカ株式会社 窒化物系セラミックス樹脂複合体

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2023190559A1 (ja) * 2022-03-30 2023-10-05 デンカ株式会社 放熱構造体

Also Published As

Publication number Publication date
JPWO2021200967A1 (cg-RX-API-DMAC7.html) 2021-10-07

Similar Documents

Publication Publication Date Title
JP6285155B2 (ja) 放熱部材およびその用途
WO2021200966A1 (ja) 窒化ホウ素焼結体及び複合体、並びに放熱部材
CN111499391A (zh) 树脂浸渗氮化硼烧结体及其用途
JP7566883B2 (ja) 窒化ホウ素焼結体、複合体及びこれらの製造方法、並びに放熱部材
JP7510497B2 (ja) 複合体の製造方法
JP7550869B2 (ja) 複合体及びその製造方法、並びに、積層体及びその製造方法
WO2020203692A1 (ja) 複合体
WO2020203688A1 (ja) 複合体の製造方法
JP7598925B2 (ja) 窒化ホウ素焼結体、複合体及びこれらの製造方法、並びに放熱部材
WO2022209325A1 (ja) 複合体及びその製造方法、樹脂充填板、並びに、積層体及びその製造方法
WO2021230328A1 (ja) 複合体及び積層体
WO2021200973A1 (ja) 複合体の製造方法
JP7458479B2 (ja) 複合体及び複合体の製造方法
WO2021200971A1 (ja) 窒化ホウ素焼結体、複合体及びこれらの製造方法、並びに放熱部材
WO2021200719A1 (ja) 窒化ホウ素焼結体、複合体及びこれらの製造方法、並びに放熱部材
WO2022071247A1 (ja) 複合シート及びその製造方法、並びに、積層体及びその製造方法
JP7165844B2 (ja) 複合シート及びその製造方法、並びに、積層体及びその製造方法
JP2025085032A (ja) 複合体及びその製造方法、並びに、接合体、回路基板及びパワーモジュール
JP7319482B2 (ja) セラミックス板の製造方法、セラミックス板、複合シート、及び積層基板
WO2022071293A1 (ja) 複合シート及びその製造方法、積層体及びその製造方法、並びに、パワーデバイス
WO2022071294A1 (ja) 複合体の接着信頼性及び放熱性能を評価する方法、及び複合体

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 21781519

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2022512550

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 21781519

Country of ref document: EP

Kind code of ref document: A1