WO2021188226A1 - Planarization of spin-on films - Google Patents

Planarization of spin-on films Download PDF

Info

Publication number
WO2021188226A1
WO2021188226A1 PCT/US2021/017165 US2021017165W WO2021188226A1 WO 2021188226 A1 WO2021188226 A1 WO 2021188226A1 US 2021017165 W US2021017165 W US 2021017165W WO 2021188226 A1 WO2021188226 A1 WO 2021188226A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
substrate
pattern
device features
actinic radiation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2021/017165
Other languages
English (en)
French (fr)
Inventor
Anthony R. SCHEPIS
Anton Devilliers
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tokyo Electron Ltd
Tokyo Electron US Holdings Inc
Original Assignee
Tokyo Electron Ltd
Tokyo Electron US Holdings Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tokyo Electron Ltd, Tokyo Electron US Holdings Inc filed Critical Tokyo Electron Ltd
Priority to KR1020227035158A priority Critical patent/KR102901242B1/ko
Priority to JP2022555939A priority patent/JP7812040B2/ja
Priority to CN202180021194.1A priority patent/CN115298805B/zh
Publication of WO2021188226A1 publication Critical patent/WO2021188226A1/en
Anticipated expiration legal-status Critical
Priority to JP2025133001A priority patent/JP2025159084A/ja
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P95/00—Generic processes or apparatus for manufacture or treatments not covered by the other groups of this subclass
    • H10P95/06—Planarisation of inorganic insulating materials
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P76/00—Manufacture or treatment of masks on semiconductor bodies, e.g. by lithography or photolithography
    • H10P76/20—Manufacture or treatment of masks on semiconductor bodies, e.g. by lithography or photolithography of masks comprising organic materials
    • H10P76/204—Manufacture or treatment of masks on semiconductor bodies, e.g. by lithography or photolithography of masks comprising organic materials of organic photoresist masks
    • H10P76/2041—Photolithographic processes
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/63—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the formation processes
    • H10P14/6326—Deposition processes
    • H10P14/6342—Liquid deposition, e.g. spin-coating, sol-gel techniques or spray coating
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/65—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by treatments performed before or after the formation of the materials
    • H10P14/6516—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by treatments performed before or after the formation of the materials of treatments performed after formation of the materials
    • H10P14/6536—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by treatments performed before or after the formation of the materials of treatments performed after formation of the materials by exposure to radiation, e.g. visible light
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/68—Organic materials, e.g. photoresists
    • H10P14/683—Organic materials, e.g. photoresists carbon-based polymeric organic materials, e.g. polyimides, poly cyclobutene or PVC
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/69—Inorganic materials
    • H10P14/692—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses
    • H10P14/6921—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses containing silicon
    • H10P14/6922—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses containing silicon the material containing Si, O and at least one of H, N, C, F or other non-metal elements, e.g. SiOC, SiOC:H or SiONC
    • H10P14/6925—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses containing silicon the material containing Si, O and at least one of H, N, C, F or other non-metal elements, e.g. SiOC, SiOC:H or SiONC the material comprising hydrogen silsesquioxane, e.g. HSQ
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P95/00—Generic processes or apparatus for manufacture or treatments not covered by the other groups of this subclass
    • H10P95/08—Planarisation of organic insulating materials
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D1/00—Processes for applying liquids or other fluent materials
    • B05D1/002—Processes for applying liquids or other fluent materials the substrate being rotated
    • B05D1/005—Spin coating
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P74/00—Testing or measuring during manufacture or treatment of wafers, substrates or devices
    • H10P74/20—Testing or measuring during manufacture or treatment of wafers, substrates or devices characterised by the properties tested or measured, e.g. structural or electrical properties
    • H10P74/203—Structural properties, e.g. testing or measuring thicknesses, line widths, warpage, bond strengths or physical defects

Definitions

  • This disclosure relates to semiconductor fabrication and related processes, including planarization of spin-on films.
  • Semiconductor processing involves forming many layers of materials over a semiconductor substrate. Some integration schemes may involve 70 or more levels to a design. Each level includes multiple process steps that involve the patterning of various films with differing geometries and aspect ratios. These patterning processes may result in non-planar topography that can impact the integrity of spin-on films used in standard semiconductor device processes.
  • Photoresist is a fundamental spin-on material used to pattern the majority of semiconductor layers employing lithography. It is important for a photoresist film to be applied uniformly to the wafer as changes in material thickness significantly hinder critical dimension resolution of a lithography process. Uniform application of photoresist films can be difficult, however, with topography. This is because the mechanics of the spin-on process cause vaiying thickness or coat defects as the resist interacts with features of varying heights/ depths.
  • a method of forming a device includes receiving a substrate having microfabricated structures that differ in height relative to each other in a direction perpendicular to a working surface of the substrate such that the microfabricated structures define a non-planar topography across the working surface of the substrate; depositing a first layer on the working surface of the substrate by spin-on deposition, the first layer including a solubility-shifting agent, depositing the first layer resulting in a non-planar film; exposing the first layer to a first pattern of actinic radiation, the first pattern of actinic radiation based on a topography of the substrate, the first pattern of actinic radiation changing a solubility of the first layer such that upper regions of non-planar topography of the first layer are soluble to a predetermined solvent, and lower regions of non-planar topography of the first layer are insoluble to the predetermined solvent; developing the first layer using the predetermined solvent such that soluble portions of the first layer are removed; and depositing
  • a method of forming a device includes receiving a substrate having a non-planar surface in that the substrate has first surfaces and second surfaces, the first surfaces having a greater z-height as compared to the second surfaces; depositing a first layer on the working surface of the substrate by spin- on deposition, the first layer including a solubility-shifting agent, depositing the first layer resulting in a non-planar film in that the first layer covers both the first surfaces and the second surfaces; exposing the first layer to a first pattern of actinic radiation, the first pattern of actinic radiation based on coordinate locations of the first surfaces and the second surfaces, the first pattern of actinic radiation changing a solubility of the first layer such portions of the first layer that are on the first surfaces are soluble to a predetermined solvent, and portions of the first layer that are on the second surfaces are insoluble to the predetermined solvent; developing the first layer using the predetermined solvent such that soluble portions of the first layer are removed; and depositing
  • a method of forming a device includes receiving a substrate including a first set of device features and a second set of device features formed across a major surface of the substrate, the first set of device features having a greater height than the second set of device features, where a height difference between the first set of device features and the second set of device features form a non-planar topography across the major surface of the substrate; spin-coating a first intervening layer over the substrate; exposing the substrate to a first localized pattern of radiation, where the first localized pattern of radiation is projected using direct write lithography; developing the first intervening layer to reduce the height difference between the first set of device features and the second set of device features; and measuring a topographic metric across the major surface of the substrate.
  • Figures 1A-1D illustrate cross-sectional views of a semiconductor device during various stages of fabrication in accordance with an embodiment of the present application, wherein Figure lA illustrates a semiconductor device having a non-planar topography
  • Figure lB illustrates the device after depositing a first intervening layer and exposing the first intervening layer to a pattern of radiation
  • Figure 1C illustrates the device after developing the first intervening layer
  • Figure lD illustrates the device after coating the material with a second material
  • Figure 2 is a flow chart of a method for planarizing the working surface of a substrate according to an embodiment of the present invention
  • Figures 3A-3B illustrate cross-sectional view of a semiconductor device during various stages of fabrication according to an embodiment of the present application, wherein Figure 3A illustrates a semiconductor device after exposing a second intervening layer to a pattern of radiation, and Figure 3B illustrates the device after developing the second intervening layer.
  • topographies directly influences processing of semiconductor devices, specifically spin-on films.
  • One such film is photoresist, a fundamental spin-on material used to pattern the majority of semiconductor layers employing lithography.
  • photoresist a fundamental spin-on material used to pattern the majority of semiconductor layers employing lithography.
  • interaction with topography can create thickness variations across the wafer. These thickness variations may create problems for subsequent steps in a semiconductor fabrication process.
  • lithographic imaging is generally used as part of a process to pattern surfaces of a semiconductor device during fabrication.
  • An example of a lithographic process includes depositing photoresist on a substrate, partially exposing the photoresist to light through a patterned etch mask, developing the exposed photoresist to define the mask pattern in the photoresist, and then etching the photoresist to form the pattern in the substrate.
  • a photoresist film It is important for a photoresist film to be applied uniformly to the substrate as changes in material thickness significantly hinder critical dimension resolution of a lithography process.
  • the critical dimension resolution of a pattern of features depends on the height variability of the film thickness of the photoresist. Lithography exposure systems are sensitive to focus changes. As the thickness of the photoresist changes across the surface of the substrate, so does the integrity of the subsequent pattern of features being resolved. Thus, a non-planar layer of the photoresist can induce variability in the critical dimension, thickness, profiles and/or roughness of a pattern of features being imaged. It is typically important for the definition of a pattern of device features to be uniform as their dimensionality impacts device performance/yield. [0015] Embodiments of this disclosure describe a method for planarizing a non-planar surface across a substrate for subsequent lithographic patterning.
  • Embodiments of this disclosure include improved techniques for planarizing a film deposited over a substrate having a varied topography. Embodiments of this disclosure include applying intervening layers across a substrate and selectable exposing of the intervening layers to improve the planarity of a substrate.
  • Figures 1A-1D illustrate cross-sectional views of a semiconductor device during various stages of fabrication in accordance with an embodiment of the present application, wherein Figure lA illustrates a semiconductor device having a non-planar topography
  • Figure lB illustrates the device after depositing a first intervening layer and exposing the first intervening layer to a pattern of radiation
  • Figure lC illustrates the device after developing the first intervening layer
  • Figure lD illustrates the device after coating the material with a second material.
  • a semiconductor device too has a non-planar topography that includes microfabricated structures.
  • the microfabricated structures may include structures 104 that define recesses 106 and top surfaces 108 across a working surface of a substrate 102.
  • this disclosure describes “recesses” it will be appreciated that other suitable features might be formed in a semiconductor layer, including lines, holes, open areas, trenches, vias, and/or other suitable structures. Structures 104 and recesses 106 may be formed using conventional lithography processes.
  • Substrate 102 generically refers to a workpiece being processed in accordance with embodiments of the invention.
  • the substrate 102 may include any material portion or structure of a device, particularly a semiconductor or other electronics device, and may, for example, be a base substrate structure, such as a semiconductor wafer, reticle, or a layer on or overlying a base substrate structure such as a thin film.
  • substrate 102 is not limited to any particular base structure, underlying layer or overlying layer, patterned or un patterned, but rather, is contemplated to include any such layer or base structure, and any combination of layers and/or base structures.
  • the substrate 102 may be a bulk substrate such as a bulk silicon substrate, a silicon on insulator substrate, or various other semiconductor substrates including a germanium substrate, a silicon carbide substrate, a gallium nitride (GaN) substrate including GaN on silicon, a gallium arsenide substrate, and others.
  • a bulk substrate such as a bulk silicon substrate, a silicon on insulator substrate, or various other semiconductor substrates including a germanium substrate, a silicon carbide substrate, a gallium nitride (GaN) substrate including GaN on silicon, a gallium arsenide substrate, and others.
  • the microfabricated structures differ in height relative to each other.
  • the recesses have a first height 103 and the structures 104 and top surfaces 108 have a second height 105 in the z- direction.
  • the height difference of microfabricated structures relative to each other maybe between 10 nm and too nm, e.g., greater than 50 nm. In other embodiments, the height difference may be greater than 5 microns especially in case of a deep opening / trench.
  • the height (or depth) of each of the microfabricated structures may be measured using, scanning electron microscopy (SEM), small angle x-ray scattering (SAXS), or wafer optical scatterometry.
  • Figure lB illustrates a cross-sectional view of the semiconductor device after a first intervening layer 110 is deposited across the working surface of the substrate 102 using spin-on deposition.
  • the first intervening layer 110 may comprise a photosensitive material such as a positive, negative, or a hybrid toned photoresist.
  • the first intervening layer 110 comprises phenol formaldehyde resin or a diazo-naphthoquinone based resin.
  • the first intervening layer 110 may comprise a chemically amplified resist.
  • the first intervening layer 110 comprises a non-chemically amplified resist material such as PolyMethyl MethAcrylate (PMMA) or Hydrogene SilsesQuioxance (HSQ).
  • PMMA PolyMethyl MethAcrylate
  • HSQ Hydrogene SilsesQuioxance
  • a particular material e.g. the first intervening layer 110
  • the substrate is then rotated at a relatively high velocity, e.g., 2000 to 8000 rpm, so that centrifugal force causes the deposited material to move towards the edges of the substrate 102, thereby coating the substrate 102. Excess material is spun off the substrate 102.
  • the thickness of the photoresist is determined by, amongst other factors, the resist viscosity and rotational speed of the substrate while spinning.
  • the photoresist is baked to form the first intervening layer 110.
  • a soft bake process maybe used to evaporate the residual solvent of the photoresist and to densify the photoresist.
  • the soft bake process includes heating the photo resist within a narrow temperature range, e.g., between 75 °C and 100 °C.
  • a substrate 102 includes a non-planar topography of densely packed microfabricated structures
  • this density can push the deposited material upward and manipulate a mass fraction of how much material fills in the recesses 106.
  • the deposited material interacts with the non-planar surface of the substrate 102 (e.g., the differing heights between the microfabricated structures).
  • This causes the deposited material to be deposited with a varying film thickness (e.g., varying z-heights across the substrate).
  • the first intervening layer 110 is deposited using a spin-on deposition process resulting in a varying film thickness across the non-planar surface of the substrate 102.
  • the first intervening layer 110 may be deposited with a thicker film thickness in the recesses 106 and a thinner film thickness on the structures 104 and the top surfaces 108 (or vice versa).
  • the topography of the first intervening layer 110 is merely an example, and that actual changes in topography may vary from deposition to deposition, even with a substrate having a similar topography of substrate
  • the first intervening layer 110 is exposed to a localized radiation pattern to improve the planarization of the working surface of the substrate 102.
  • the first intervening layer 110 undergoes exposure to a localized pattern of radiation 112.
  • the substrate 102 Prior to the exposure to radiation 112, the substrate 102 is aligned with the tool exposing the substrate 102 to the radiation.
  • the alignment may depend on the stack that is being patterned.
  • metallic materials in the back end of the line may be used to align the tool.
  • optical alignment with an alignment mark may be used.
  • the topography of the first intervening layer 110 may be used to align the substrate 102.
  • the topography of the first intervening layer 110 is measured.
  • the topography of the first intervening layer may be measured using a measuring tool such as an atomic force microscopy (AFM), a profilometer, or an optical thickness metrology tool.
  • AFM atomic force microscopy
  • profilometer a profilometer
  • optical thickness metrology tool an optical thickness metrology tool
  • the exposure pattern of the pattern of radiation 112 is determined. Because the expected topography is determined by the layout, the exposure pattern can be predetermined in some embodiments. In one or more embodiments, pattern of radiation 112 is localized such that the portions of the first intervening layer 110 covering the higher/taller microfabricated structures (e.g. the structures 104 and top surfaces 108) are removed and the portions of the first intervening layer 110 filling the recesses 106 remain after a subsequent development step.
  • the pattern of radiation 112 may comprise actinic radiation such as ultraviolet radiation projected using a mask-less lithography tool, such as a direct write lithography tool.
  • direct write lithography methods such as digital light projection (DLP), grating light valve lithography, electron beam lithography, plasmonic lithography, focused ion beam (FIB) lithography or nanoimprinting may be used to form the exposure pattern of the pattern of radiation 112.
  • the pattern of radiation 112 may comprise an actinic radiation having a wavelength between 365 nm and 405 nm and may be formed and projected using a direct write lithography process in a dedicated direct writing machine.
  • the direct write lithography process uses computer controlled optics to project an exposure pattern of radiation instead of using a traditional mask.
  • Traditionally to expose a substrate to a pattern of radiation requires: designing a mask using computer aided design (CAD) software, building the mask, and exposing the substrate through the mask.
  • CAD computer aided design
  • direct write lithography utilizes computer controlled optics to project radiation, the computer controlled optics are able to form a pattern of radiation directly from the CAD file.
  • the first intervening layer 110 deposited on identical substrates may have different topographies. Therefore, to planarize identical substrates, individual patterns of radiation have to be formed.
  • direct write lithography is a mask-less radiation that allows for the pattern of radiation 112 to be programmed digitally.
  • the pattern of radiation 112 is localized over the structures 104 and the top surfaces 108.
  • the portions of the first intervening layer 110 covering the structures 104 and the top surfaces 108 become soluble to a solvent, such as developer fluid, while portions of the hrst intervening layer 110 filing the recesses 106 remain insoluble to the solvent.
  • the pattern of radiation 112 is localized over the recesses 106. In this manner the portions of the hrst intervening layer 110 covering the recesses become insoluble to a solvent while the portions of the first intervening layer no cover the structures 104 and the top surfaces 108 are soluble in the solvent.
  • a hard bake process may be performed to stabilize and harden the photoresist.
  • the hard bake process may be performed at a higher temperature than the soft bake process and, for example, performed between 100 °C and 150 °C.
  • Figure 1C illustrates the semiconductor device after portions of the first intervening layer no are removed.
  • a developing step is then executed to remove the soluble portions of the first intervening layer no deposited over the structures 104 and the top surfaces 108.
  • the first intervening layer no may be removed by exposing to a developer solution, which may comprise phenol-based strippers, acetone, trichloroethylene, and others when the first intervening layer no is a positive resist.
  • the first intervening layer no may be removed by exposing to a developer solution, which may comprise methyl ethyl ketone, methyl isobutyl ketone, and others when the first intervening layer no is a negative resist.
  • the portions of the first intervening layer no remain within the recesses 106.
  • One advantage of this is the remaining portions of the first intervening layer no decreases the relative height difference between the recesses 106 and the structures 104 and the top surfaces 108 (i.e. the first height 103 increases due to the first intervening layer). Therefore, the difference between the first height 103 and the second height 105 is reduced, resulting in an improved topography.
  • a topographic metric of the substrate may be measured.
  • the topographic metric may include, for example, the planarity or uniformity of the first intervening layer no.
  • the topographic metric may be measured using an optical metrology technique. For example, the thickness of the intervening layer no may be measured at different locations or the height of the top surface of the intervening layer no may be measured relative to a horizontal plane at different locations. The statistical distribution may be then used to obtain a measure of the planarity or uniformity of the intervening layer no.
  • Other less often used metrics for measuring topography may also include surface techniques, for example, measuring surface roughness of the substrate 102.
  • the topographic metric may be compared to a target topographic metric. In one embodiment, if the measured topographic metric meets the topographic metric, a subsequent pattern of microstructures may be formed on the substrate using a conventional lithography process. In other embodiments, if the topographic metric does not meet a target topographic metric, the process discussed above may be repeated until a target topographic metric is met.
  • a second material 114 is deposited onto the substrate using spin-on deposition. As illustrated in Figure lD, the second material 114 is deposited in a more planar fashion than the deposition of the hrst intervening layer 110.
  • the composition of the second material 114 depends on whether the target topography metric was met in the previous step. In one or more embodiments where the target topography metric was met, the second material 114 may comprise a photoresist used in a lithography process to form a subsequent pattern of microfabricated structures. In one or more embodiments, where the target topography metric was not met, the second material 114 may be a second intervening layer comprising the same material as the first intervening layer 110 intended to further planarize the working surface of the substrate 102.
  • Figure 2 is a flow chart illustrating an example process flow used to planarize a working surface of a substrate in accordance with an embodiment of the present invention.
  • a substrate 102 having microfabricated structures that differ in height relative to each other are formed across a working surface of a substrate 102.
  • the difference in height between the microfabricated structures defines a non-planar topography across the working surface of the substrate 102.
  • a first intervening layer 110 is deposited across the substrate using spin-on deposition. As next illustrated in block 204 and described with reference to Figure lB, the first intervening layer 110 is exposed to a pattern of radiation 112.
  • the first intervening layer is developed to remove the portions of the first intervening layer 110 deposited over the structures 104 and the top surfaces 108.
  • removing the portions of the first intervening layer 110 deposited over the higher surfaces while the portions of the first intervening layer 110 remain in the recesses reduces the relative heights between the microfabricated structures.
  • One advantage of this is that it improves the planarity of the working surface of the substrate 102.
  • a topographic metric across the working surface of the substrate 102 is measured.
  • the measured topographic metric is compared to a target topographic metric.
  • the target topographic metric may be a surface height relative to a horizontal plane as measured with an optical technique or an electron microscopy technique.
  • the surface height may be defined based on the tolerance levels of the process equipment being used, for example, the depth of focus of the lithography imaging tool.
  • a standard deviation of the surface height of the top surface may be compared with a target standard deviation and topologies outside the target standard deviation may be marked as not meeting the topographic metric.
  • the target topographic measurement may be defined as the uniformity of the first intervening layer 110..
  • the planarity or uniformity of the first intervening layer 110 may be measured using an optical metrology technique. If the measured topographic metric meets a target topographic metric, the method proceeds to block 212 and a subsequent pattern of microstructures maybe formed on the substrate 102 using a conventional lithography process.
  • a topographic metric of the subsequent pattern of microfabricated devices is compared to a threshold topographic metric.
  • the process proceeds to block 214.
  • an additional intervening layer is deposited over the substrate using spin-on deposition.
  • the additional intervening layer may comprise the same material as the first intervening layer 110. After depositing the additional intervening layer, the method repeats blocks 204-212 until the target topographic metric is met.
  • Figures 3A-3B illustrate an example of further planarizing the substrate if the measured topographic metric does not meet the target topographic metric. Accordingly, Figures 3A-3C continues from Figures 1A-1D.
  • Figures 3A-3B illustrate cross-sectional view of a semiconductor device during various stages of fabrication according to an embodiment of the present application, where Figure 3A illustrates a semiconductor device after exposing a second intervening layer to a pattern of radiation, and Figure 3B illustrates the device after developing the second intervening layer.
  • a second intervening layer 314 is deposited over the substrate using spin on deposition and is exposed to a pattern of radiation 112. As illustrated in Figure 3A, the second intervening layer 314 is deposited with an improved planarity compared to when the first intervening layer 110 was deposited due to the decrease in the relative height difference between the microstructures.
  • the second intervening layer 314 may comprise the same material as the first intervening layer 110.
  • the pattern of radiation may comprise the same material and may be formed in the same manner described in Figure lB.
  • the second intervening layer 314 undergoes a development step to remove the portions of the second intervening layer 314 covering the structures 104 and the top surfaces 108.
  • the development step may comprise the same material and may be performed in the same manner described in Figure 1C.
  • the relative height difference between the recesses 106 and the structures 104 and the top surfaces 108 is further reduced by the second intervening layer 314. This results in the substrate 102 having a further improved planarization.
  • Example 1 A method of planarizing a substrate, the method including: receiving a substrate having microfabricated structures that differ in height relative to each other in a direction perpendicular to a working surface of the substrate such that the microfabricated structures define a non-planar topography across the working surface of the substrate; depositing a first layer on the working surface of the substrate by spin-on deposition, the first layer including a solubility-shifting agent, depositing the first layer resulting in a non-planar film; exposing the first layer to a first pattern of actinic radiation, the first pattern of actinic radiation based on a topography of the substrate, the first pattern of actinic radiation changing a solubility of the hrst layer such that upper regions of non-planar topography of the first layer are soluble to a predetermined solvent, and lower regions of non-planar topography of the hrst layer are insoluble to the predetermined solvent; developing the first layer using the predetermined solvent such that soluble portions of the first layer are removed; and depositing a first layer
  • Example 2 The method of example 1, where the first pattern of actinic radiation is projected using a direct-write system.
  • Example 3 The method of one of examples 1 or 2, where the microfabricated structures have relative height differences greater than hve microns.
  • Example 4 The method of one of examples 1 to 3, where the microfabricated structures have relative height differences greater than 50 nanometers.
  • Example 5 The method of one of examples 1 to 4, further including: where the second layer includes the solubility-shifting component; exposing the second layer to the first pattern of actinic radiation, the first pattern of actinic radiation changing a solubility of the second layer such that upper regions of the second layer are soluble to a predetermined solvent, and lower regions of the second layer are insoluble to the predetermined solvent; and developing the second layer using the predetermined solvent such that soluble portions of the first layer are removed.
  • Example 6 A method of planarizing a substrate, the method including: receiving a substrate having a non-planar surface in that the substrate has first surfaces and second surfaces, the first surfaces having a greater z-height as compared to the second surfaces; depositing a first layer on the working surface of the substrate by spin-on deposition, the first layer including a solubility-shifting agent, depositing the first layer resulting in a non-planar film in that the first layer covers both the first surfaces and the second surfaces; exposing the first layer to a first pattern of actinic radiation, the first pattern of actinic radiation based on coordinate locations of the first surfaces and the second surfaces, the first pattern of actinic radiation changing a solubility of the first layer such portions of the first layer that are on the first surfaces are soluble to a predetermined solvent, and portions of the first layer that are on the second surfaces are insoluble to the predetermined solvent; developing the first layer using the predetermined solvent such that soluble portions of the first layer are removed; and depositing a second layer on
  • Example 7 The method of example 6 where the first pattern of actinic radiation is projected using a direct-write system.
  • Example 8 The method of one of examples 6 or 7 further including: exposing the second layer to the first pattern of actinic radiation, the first pattern of actinic radiation based on coordinate locations of the first surfaces and the second surfaces, the first pattern of actinic radiation changing a solubility of the second layer such that portions of the second layer that are on the first surfaces are soluble to the predetermined solvent, and portions of the second layer that are on the second surfaces are insoluble to the predetermined solvent; and developing the second layer using the predetermined solvent such that soluble portions of the second layer are removed.
  • Example 9 The method of one of examples 6 to 8, where the first surfaces have a z-height greater than at least 5 microns compared to the second surfaces.
  • Example 10 The method of one of examples 6 to 9, where the first surfaces have a z-height greater than at least 50 nm compared to the second surfaces.
  • Example n The method of one of examples 6 to 10, where the first pattern of actinic radiation has a wavelength between 193 nm and 405 nm.
  • Example 12 A method for forming a device, the method including: receiving a substrate including a first set of device features and a second set of device features formed across a major surface of the substrate, the first set of device features having a greater height than the second set of device features, where a height difference between the first set of device features and the second set of device features form a non-planar topography across the major surface of the substrate; spin-coating a first intervening layer over the substrate; exposing the substrate to a first localized pattern of radiation, where the first localized pattern of radiation is projected using direct write lithography; developing the first intervening layer to reduce the height difference between the first set of device features and the second set of device features; and measuring a topographic metric across the major surface of the substrate.
  • Example 13 The method of example 12 further including: comparing the topographic metric to a target topographic metric; in response to determining the topographic metric meets the target topographic metric, forming a subsequent pattern of device features using a conventional lithography process.
  • Example 14 The method of one of examples 12 or 13 further including: comparing the topographic metric to a target topographic metric; and in response to determining the topographic metric is different from a target topographic metric, spin coating a second intervening layer over the substrate, exposing the substrate to the localized pattern of radiation, and developing the second intervening layer to further reduce the height difference between the first set of device features and the second set of device features.
  • Example 15 The method of one of examples 12 to 14, where the first intervening layer includes a positive tone photoresist and the localized pattern of radiation is formed over the first set of device features.
  • Example 16 The method of one of examples 12 to 15, where the first intervening layer includes a negative tone photoresist and the localized pattern of radiation is formed over the second set of device features.
  • Example 17 The method of one of examples 12 to 16, where the first radiation includes of actinic radiation.
  • Example 18 The method of one of examples 12 to 17, where the first radiation has a wavelength between 193 nm and 405 nm.
  • Example 19 The method of one of examples 12 to 18, where the height difference between the first set of device features and the second set of device features is greater than five microns.
  • Example 20 The method of one of examples 12 to 19, where the height difference between the first set of device features and the second set of device features is greater than 50 nm.

Landscapes

  • Exposure And Positioning Against Photoresist Photosensitive Materials (AREA)
  • Photosensitive Polymer And Photoresist Processing (AREA)
  • Exposure Of Semiconductors, Excluding Electron Or Ion Beam Exposure (AREA)
PCT/US2021/017165 2020-03-17 2021-02-09 Planarization of spin-on films Ceased WO2021188226A1 (en)

Priority Applications (4)

Application Number Priority Date Filing Date Title
KR1020227035158A KR102901242B1 (ko) 2020-03-17 2021-02-09 스핀-온 막의 평탄화
JP2022555939A JP7812040B2 (ja) 2020-03-17 2021-02-09 スピンオン膜の平坦化
CN202180021194.1A CN115298805B (zh) 2020-03-17 2021-02-09 旋涂薄膜的平坦化
JP2025133001A JP2025159084A (ja) 2020-03-17 2025-08-08 スピンオン膜の平坦化

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
US202062990823P 2020-03-17 2020-03-17
US62/990,823 2020-03-17
US17/122,898 US11776808B2 (en) 2020-03-17 2020-12-15 Planarization of spin-on films
US17/122,898 2020-12-15

Publications (1)

Publication Number Publication Date
WO2021188226A1 true WO2021188226A1 (en) 2021-09-23

Family

ID=77748471

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2021/017165 Ceased WO2021188226A1 (en) 2020-03-17 2021-02-09 Planarization of spin-on films

Country Status (6)

Country Link
US (1) US11776808B2 (cg-RX-API-DMAC7.html)
JP (2) JP7812040B2 (cg-RX-API-DMAC7.html)
KR (1) KR102901242B1 (cg-RX-API-DMAC7.html)
CN (1) CN115298805B (cg-RX-API-DMAC7.html)
TW (1) TWI896615B (cg-RX-API-DMAC7.html)
WO (1) WO2021188226A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN114744065A (zh) * 2022-03-23 2022-07-12 中国电子科技集团公司第十一研究所 台面结构芯片的非接触式光刻方法

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US12325046B2 (en) * 2022-06-28 2025-06-10 Canon Kabushiki Kaisha Superstrate including a body and layers and methods of forming and using the same

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR970030396A (ko) * 1995-11-29 1997-06-26 김광호 반도체 장치의 평탄화 방법
US20010006761A1 (en) * 1998-09-28 2001-07-05 John Golz Method and apparatus for resist planarization
US6645851B1 (en) * 2002-09-17 2003-11-11 Taiwan Semiconductor Manufacturing Company Method of forming planarized coatings on contact hole patterns of various duty ratios
US20120266810A1 (en) * 2011-04-20 2012-10-25 Taiwan Semiconductor Manufacturing Company, Ltd. Planarization system for high wafer topography
US20160300726A1 (en) * 2015-04-13 2016-10-13 Tokyo Electron Limited System and Method for Planarizing a Substrate

Family Cites Families (14)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20090008579A1 (en) * 2003-10-07 2009-01-08 Tokyo Electron Limited Electron beam lithography apparatus and design method of patterned beam-defining aperture
US7229745B2 (en) * 2004-06-14 2007-06-12 Bae Systems Information And Electronic Systems Integration Inc. Lithographic semiconductor manufacturing using a multi-layered process
JP2006049684A (ja) * 2004-08-06 2006-02-16 Sanyo Electric Co Ltd 半導体装置の製造方法
KR100612027B1 (ko) * 2005-05-12 2006-08-11 삼성전자주식회사 가교 폴리머를 이용한 잉크젯 프린트헤드의 제조방법
US7419611B2 (en) * 2005-09-02 2008-09-02 International Business Machines Corporation Processes and materials for step and flash imprint lithography
KR20160083080A (ko) * 2013-11-08 2016-07-11 도쿄엘렉트론가부시키가이샤 화학적 폴리싱 및 평탄화를 위한 방법
WO2017087066A1 (en) * 2015-11-20 2017-05-26 Tokyo Electron Limited Methods of forming etch masks for sub-resolution substrate patterning
KR102399364B1 (ko) * 2016-10-04 2022-05-18 도쿄엘렉트론가부시키가이샤 기판 제조 동안의 피처 토포그래피에 대한 스핀 코트 평탄화의 용이화
US10790146B2 (en) * 2016-12-05 2020-09-29 Rohm And Haas Electronic Materials Llc Aromatic resins for underlayers
US10991594B2 (en) * 2018-06-22 2021-04-27 Tokyo Electron Limited Method for area-selective etching of silicon nitride layers for the manufacture of microelectronic workpieces
US20200328102A1 (en) 2019-04-15 2020-10-15 Tokyo Electron Limited Method for die-level unique authentication and serialization of semiconductor devices
US20210294148A1 (en) * 2020-03-17 2021-09-23 Tokyo Electron Limited Planarizing Organic Films
US11455436B2 (en) * 2020-03-25 2022-09-27 Tokyo Electron Limited Predicting across wafer spin-on planarization over a patterned topography
US11656550B2 (en) * 2020-09-01 2023-05-23 Tokyo Electron Limited Controlling semiconductor film thickness

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR970030396A (ko) * 1995-11-29 1997-06-26 김광호 반도체 장치의 평탄화 방법
US20010006761A1 (en) * 1998-09-28 2001-07-05 John Golz Method and apparatus for resist planarization
US6645851B1 (en) * 2002-09-17 2003-11-11 Taiwan Semiconductor Manufacturing Company Method of forming planarized coatings on contact hole patterns of various duty ratios
US20120266810A1 (en) * 2011-04-20 2012-10-25 Taiwan Semiconductor Manufacturing Company, Ltd. Planarization system for high wafer topography
US20160300726A1 (en) * 2015-04-13 2016-10-13 Tokyo Electron Limited System and Method for Planarizing a Substrate

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN114744065A (zh) * 2022-03-23 2022-07-12 中国电子科技集团公司第十一研究所 台面结构芯片的非接触式光刻方法

Also Published As

Publication number Publication date
CN115298805B (zh) 2026-07-24
US11776808B2 (en) 2023-10-03
CN115298805A (zh) 2022-11-04
KR102901242B1 (ko) 2025-12-16
US20210296121A1 (en) 2021-09-23
TWI896615B (zh) 2025-09-11
JP2023517747A (ja) 2023-04-26
TW202208995A (zh) 2022-03-01
KR20220154724A (ko) 2022-11-22
JP2025159084A (ja) 2025-10-17
JP7812040B2 (ja) 2026-02-09

Similar Documents

Publication Publication Date Title
JP5059608B2 (ja) リバーストーン処理を利用したリセス構造の形成方法
US7357876B2 (en) Eliminating printability of sub-resolution defects in imprint lithography
US10354959B2 (en) Mark forming method, mark detecting method, and device manufacturing method using self-assembled block copolymer
JP4990479B2 (ja) 多層リソグラフィープロセスに関する新規な平坦化方法
JP2025159084A (ja) スピンオン膜の平坦化
US20110143271A1 (en) Pattern generating method and process determining method
JP6357231B2 (ja) 化学的研磨平坦化の方法
JP6057983B2 (ja) リソグラフィプロセス
US20210303741A1 (en) Predicting across wafer spin-on planarization over a patterned topography
KR20180098138A (ko) 기존 토포그래피 위에 평탄화된 에칭 마스크 구조를 형성하는 방법
JP5848386B2 (ja) インサイチュ嵌込み構造物形成方法
US7323417B2 (en) Method of forming a recessed structure employing a reverse tone process
JP5067848B2 (ja) パターンの形成方法
JP4861044B2 (ja) 基板の加工方法、パターン領域を有する部材の製造方法
JP2016212393A (ja) フォトマスクの製造方法、フォトマスク、並びにそれを用いた側壁角度測定装置及びその校正方法
KR20080086693A (ko) 반도체 소자의 오버레이 측정 방법
KR100866681B1 (ko) 반도체 소자의 패턴 형성방법
JP6631271B2 (ja) インプリントモールドの製造方法
Rangelow et al. Lithography and reactive ion etching in microfabrication
CN117912938A (zh) 一种双重图形化的方法、半导体器件及电子设备
Craven Imaging and Resist Technologies for the Micromachining Industry
JPH04100229A (ja) 半導体装置の製造方法
KR20090036013A (ko) 노광 마스크, 그의 형성 방법 및 그를 이용한 반도체 소자형성 방법
KR19990005817A (ko) 반도체장치의 미세패턴 형성방법

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 21772639

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2022555939

Country of ref document: JP

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 20227035158

Country of ref document: KR

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 21772639

Country of ref document: EP

Kind code of ref document: A1