WO2019167420A1 - Plaque de polarisation et son procédé de fabrication - Google Patents

Plaque de polarisation et son procédé de fabrication Download PDF

Info

Publication number
WO2019167420A1
WO2019167420A1 PCT/JP2018/048393 JP2018048393W WO2019167420A1 WO 2019167420 A1 WO2019167420 A1 WO 2019167420A1 JP 2018048393 W JP2018048393 W JP 2018048393W WO 2019167420 A1 WO2019167420 A1 WO 2019167420A1
Authority
WO
WIPO (PCT)
Prior art keywords
polarizing plate
polarizer
light
adhesive
irradiation
Prior art date
Application number
PCT/JP2018/048393
Other languages
English (en)
Japanese (ja)
Inventor
山崎 達也
Original Assignee
日東電工株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 日東電工株式会社 filed Critical 日東電工株式会社
Priority to CN201880090377.7A priority Critical patent/CN111788502B/zh
Priority to KR1020207015925A priority patent/KR20200123773A/ko
Publication of WO2019167420A1 publication Critical patent/WO2019167420A1/fr

Abstract

La présente invention concerne une plaque de polarisation en feuille (10) dotée d'un film transparent (31, 32) sur au moins une surface d'un polariseur à base d'alcool polyvinylique (21). Le polariseur est de préférence dénaturé par irradiation d'une surface d'extrémité de la plaque de polarisation obtenue par découpe pour obtenir une feuille avec un faisceau lumineux ayant une longueur d'onde dans laquelle le faisceau lumineux peut être absorbé par le polariseur. Un rapport A3300/A1089 d'une absorbance A3300 d'un pic à environ 3 300 cm-1 sur une absorbance A1089 d'un pic à environ 1 089 cm-1 dans un spectre d'absorption de l'infrarouge au niveau d'une partie extrémité dans une surface du polariseur ayant été soumise à la dénaturation est de préférence inférieur à A3300/A1089 dans le spectre d'absorption de l'infrarouge au niveau de la partie centrale de la surface.
PCT/JP2018/048393 2018-02-28 2018-12-27 Plaque de polarisation et son procédé de fabrication WO2019167420A1 (fr)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN201880090377.7A CN111788502B (zh) 2018-02-28 2018-12-27 偏振片及其制造方法
KR1020207015925A KR20200123773A (ko) 2018-02-28 2018-12-27 편광판 및 그 제조 방법

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2018034602A JP7013279B2 (ja) 2018-02-28 2018-02-28 偏光板およびその製造方法
JP2018-034602 2018-02-28

Publications (1)

Publication Number Publication Date
WO2019167420A1 true WO2019167420A1 (fr) 2019-09-06

Family

ID=67804921

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2018/048393 WO2019167420A1 (fr) 2018-02-28 2018-12-27 Plaque de polarisation et son procédé de fabrication

Country Status (5)

Country Link
JP (1) JP7013279B2 (fr)
KR (1) KR20200123773A (fr)
CN (1) CN111788502B (fr)
TW (1) TW201944104A (fr)
WO (1) WO2019167420A1 (fr)

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2021043370A (ja) * 2019-09-12 2021-03-18 住友化学株式会社 偏光子

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2012173588A (ja) * 2011-02-23 2012-09-10 Nitto Denko Corp 偏光板およびその製造方法
US20140175684A1 (en) * 2012-12-20 2014-06-26 Apple Inc. Methods and Equipment for Trimming Polarizers in Displays
JP2015225113A (ja) * 2014-05-26 2015-12-14 リコー光学株式会社 光学素子、成形型、製造方法及び光学装置
JP2017151162A (ja) * 2016-02-22 2017-08-31 住友化学株式会社 偏光板及び画像表示装置
JP2017151164A (ja) * 2016-02-22 2017-08-31 住友化学株式会社 偏光板及び画像表示装置

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP4170015B2 (ja) * 2002-04-18 2008-10-22 株式会社クラレ 偏光板
JP4762320B2 (ja) * 2009-02-20 2011-08-31 住友化学株式会社 液晶表示装置
JP2011022202A (ja) 2009-07-13 2011-02-03 Sumitomo Chemical Co Ltd 偏光板およびそれを用いた画像表示装置
JP5917834B2 (ja) * 2010-06-28 2016-05-18 日東電工株式会社 光学フィルム用粘着剤層、粘着型光学フィルムおよび画像表示装置

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2012173588A (ja) * 2011-02-23 2012-09-10 Nitto Denko Corp 偏光板およびその製造方法
US20140175684A1 (en) * 2012-12-20 2014-06-26 Apple Inc. Methods and Equipment for Trimming Polarizers in Displays
JP2015225113A (ja) * 2014-05-26 2015-12-14 リコー光学株式会社 光学素子、成形型、製造方法及び光学装置
JP2017151162A (ja) * 2016-02-22 2017-08-31 住友化学株式会社 偏光板及び画像表示装置
JP2017151164A (ja) * 2016-02-22 2017-08-31 住友化学株式会社 偏光板及び画像表示装置

Also Published As

Publication number Publication date
KR20200123773A (ko) 2020-10-30
CN111788502A (zh) 2020-10-16
CN111788502B (zh) 2022-11-01
JP7013279B2 (ja) 2022-01-31
JP2019148744A (ja) 2019-09-05
TW201944104A (zh) 2019-11-16

Similar Documents

Publication Publication Date Title
JP6495374B2 (ja) 画像表示装置用の偏光板、画像表示装置及び画像表示装置用の偏光板の製造方法
KR101949112B1 (ko) 편광판
CN108431650B (zh) 光学膜的制造方法
KR20150073201A (ko) 광학 필름의 제조 방법, 광학 필름 및 화상 표시 장치
JP6296107B2 (ja) 積層フィルム、積層フィルムの製造方法、偏光性積層フィルムの製造方法、偏光板の製造方法
KR20160076435A (ko) 편광판 및 그 제조 방법, 그리고 편광판의 세트, 액정 패널, 액정 표시 장치
CN107102390B (zh) 偏振板以及图像显示装置
KR20190033505A (ko) 편광판의 제조 방법
WO2019167420A1 (fr) Plaque de polarisation et son procédé de fabrication
WO2021049216A1 (fr) Procédé de production de plaque de polarisation
JP2024009307A (ja) 偏光子
CN109283608B (zh) 光学片
CN108983342B (zh) 光学膜的制造方法
KR20200007531A (ko) 편광판의 가공 방법
CN112969940A (zh) 偏振板
WO2022191246A1 (fr) Plaque de polarisation et son procédé de production
WO2023189810A1 (fr) Film polarisant, film polarisant stratifié, écran d'affichage d'image et dispositif d'affichage d'image
WO2023189811A1 (fr) Film polarisant, film polarisant stratifié, écran d'affichage d'image et dispositif d'affichage d'image
JP2022140346A (ja) 偏光板およびその製造方法
KR20220022410A (ko) 반사방지용 편광판 및 이를 포함하는 화상표시장치
KR20220022411A (ko) 반사방지용 편광판 및 이를 포함하는 화상표시장치
CN116917781A (zh) 偏振板及其制造方法
WO2023189815A1 (fr) Film polarisant et dispositif d'affichage d'image
TW202413999A (zh) 偏光薄膜、積層偏光薄膜、影像顯示面板、及影像顯示裝置
TW202231459A (zh) 積層體

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 18908004

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 18908004

Country of ref document: EP

Kind code of ref document: A1