JP3688022B2 - 六方晶窒化ほう素焼結体 - Google Patents

六方晶窒化ほう素焼結体 Download PDF

Info

Publication number
JP3688022B2
JP3688022B2 JP20329795A JP20329795A JP3688022B2 JP 3688022 B2 JP3688022 B2 JP 3688022B2 JP 20329795 A JP20329795 A JP 20329795A JP 20329795 A JP20329795 A JP 20329795A JP 3688022 B2 JP3688022 B2 JP 3688022B2
Authority
JP
Japan
Prior art keywords
sintered body
density
powder
purity
bending strength
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP20329795A
Other languages
English (en)
Other versions
JPH0952771A (ja
Inventor
裕幸 原
一成 大津
信行 吉野
美幸 中村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Denka Co Ltd
Original Assignee
Denki Kagaku Kogyo KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Denki Kagaku Kogyo KK filed Critical Denki Kagaku Kogyo KK
Priority to JP20329795A priority Critical patent/JP3688022B2/ja
Publication of JPH0952771A publication Critical patent/JPH0952771A/ja
Application granted granted Critical
Publication of JP3688022B2 publication Critical patent/JP3688022B2/ja
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【0001】
【発明の属する技術分野】
本発明は、高純度、高密度、高曲げ強度の六方晶窒化ほう素焼結体に関する
【0002】
六方晶窒化ほう素(h−BN)は、高耐熱性、高熱伝導性、高耐熱衝撃性、高電気絶縁性など優れた特性を有し、また数少ない易加工性のセラミックスであることから、セラミックス焼結用るつぼ、耐熱用治具、高温絶縁材として用いられているが、自己焼結性がないので他の一般的なセラミックスに比べて機械的強度が小さく、利用が拡大しない一原因となっている。
【0003】
【従来の技術】
従来、h−BN焼結体用のh−BN粉の評価は、例えば粒度、比表面積、不純物含有量などで行われているが、その評価結果とh−BN焼結体の特性、例えば焼結体密度、曲げ強度、BN純度などとの間にはあまり相関が認められず、実験と経験に頼らざるを得なかった。
【0004】
h−BN焼結体は、h−BN粉に焼結助剤を添加し、CIP後常圧焼結するか、又はホットプレス、HIPなどによって製造されている。焼結助剤としては、アルカリ金属酸化物、アルカリ土類金属酸化物、ほう素酸化物、希土類酸化物などが用いられているが、これらの添加によってBN純度が低くなり不純物による汚染、耐熱性の低下、絶縁破壊などを引き起こすので、焼結助剤の使用はできるけ少なくすることが望まれている。
【0005】
そこで、本出願人は、焼結助剤を添加せずに高純度でかつ高強度のh−BN焼結体を製造する方法として、h−BN粉末原料として粗粉h−BNと微粉h−BNを混合し、成形後、常圧焼結する方法を先に提案した(特願平6−106912号明細書)が、この方法によっても焼結体密度が低く、BN純度も99. 5%未満であり十分ではなかった。
【0006】
【発明が解決しようとする課題】
本発明の目的は、BN純度99.5重量%以上、密度1.91g/cm以上、常温曲げ強度50MPa以上を発現させたh−BN焼結体を提供することにある。
【0007】
【課題を解決する手段】
本発明者らは、前記課題を解決するために鋭意検討した結果、h−BN粉末原料として、酸素含有量が例えば1.0質量%であり、しかも圧力2700kg/cm で冷間静水圧(CIP)成形した場合の成形体密度が1.95g/cm以上となる充填性の大なるものを用いればよいこと見いだし、本発明を完成させたものである。
【0008】
すなわち、本発明は、BN純度99.5重量%以上、密度1.91g/cm以上、常温曲げ強度50MPa以上であることを特徴とするh−BN焼結体である。
【0009】
【発明の実施の形態】
以下、更に詳しく本発明について説明する。本発明において、h−BN焼結体のBN純度、密度及び常温曲げ強度を上記のように限定した理由は以下のとおりである。
【0010】
BN純度が99.5重量%未満では、B、焼結助剤、B と焼結助剤との複塩、焼結助剤の分解物などの不純物によって汚染され、h−BN焼結体本来の諸特性が劣化し機械加工性も低下する。BN純度は、h−BNをアルカリ分解後ケルダール法による水蒸気蒸留を行い、留出液中の全窒素を中和適定することによって測定することができる。
【0011】
密度が1.91g/cm 未満では、相対密度が80%未満となり、空隙の多い焼結体組織となってh−BN焼結体本来の優れた物性が低下する。密度はアルキメデス法によって測定することができる。
【0012】
常温曲げ強度が50MPa未満では、取扱い時又は加工時の割れ、クラックを引き起こす。常温曲げ強度はJIS R1601の三点曲げ強さ試験に準じて測定することができる。
【0013】
本発明のh−BN焼結体は次のようにして製造することができる。まず、原料h−BN粉末としては、圧力2700kg/cm下におけるCIP成形体密度が1.95g/cm 以上となるh−BN粉を35重量%以上(100重量%を含む)含み、酸素含有量が例えば1.0重量%である粉末が使用される。このようなh−BN粉末原料は、圧力2700kg/cm 下におけるCIP成形体密度が1.95g/cm以上で酸素含有量1.6重量%以上のh−BN粉に酸素含有量1.6重量%未満のh−BN粉を混合する方法、圧力2700kg/cm下におけるCIP成形体密度1.95g/cm以上で酸素含有量1.6重量%未満のh−BN粉に酸素含有量1.6重量%以上のh−BN粉を混合する方法などによって入手することができる。混合には振動ミル、ボールミル、リボンブレンダーなどが用いられる。
【0014】
本発明で使用される圧力2700kg/cm下におけるCIP成形体密度1.95g/cm以上となるh−BN粉は、普通一般に入手される市販のh−BN粉をジェットミル粉砕することによって得ることができる。このようなCIP成形体密度を示すh−BN粉は、h−BN粉末原料中に35重量%以上(100重量%を含む)含まれていることが好ましく、35重量%未満ではh−BN焼結体の密度が1.91g/cm以上とはならない。
【0015】
本発明において、h−BN粉末原料の酸素含有量が1.6重量%をこえるとh−BN焼結体のBN純度が99.5重量%未満となり、また0.5重量%未満では焼結が起こらず、常温曲げ強度50MPa以上のh−BN焼結体を製造することが困難となる。
【0016】
焼結方法としては一般的な焼結方法、例えばホットプレス法、常圧焼結法、HIP法などを採用することができる。焼成温度は1400℃〜2400℃が好ましく、1400℃未満では焼結が不十分となって常温曲げ強度が低下し、また2400℃をこえるとh−BNが気化又は異常粒成長を起こし、常温曲げ強度が低下する。
【0017】
【実施例】
以下、実施例、比較例をあげて更に具体的に本発明を説明する。
実施例1〜4 比較例1〜8
市販のh−BN粉又はそれをジェットミル粉砕してなる(a)〜(g)の7種のh−BN粉を準備し、それらについて圧力2700kg/cm下におけるCIP成形体密度を測定した。その結果を表1に示す。次いで、これらのh−BN粉を種々混合してh−BN粉末原料を調製し、それを黒鉛製ダイスに充填し、圧力200kg/cm、表2に示す焼成温度で1hr保持しホットプレスを行った。h−BN粉末原料の酸素含有量と平均粒径(計算値)、及び得られたh−BN焼結体について、BN純度、密度及び常温曲げ強度を測定した。それらの結果を表2に示す。
【0018】
【表1】
Figure 0003688022
【0019】
【表2】
Figure 0003688022
【0020】
【発明の効果】
本発明によれば、BN純度99.5重量%以上、密度1.91g/cm以上、常温曲げ強度50MPa以上の高純度、高密度、高曲げ強度のh−BN焼結体が提供される。

Claims (1)

  1. BN純度99.5重量%以上、密度1.91g/cm以上、常温曲げ強度50MPa以上であることを特徴とする六方晶窒化ほう素焼結体。
JP20329795A 1995-08-09 1995-08-09 六方晶窒化ほう素焼結体 Expired - Fee Related JP3688022B2 (ja)