DE2737232B2 - Verwendung von Reinaluminium für Aluminiumdosen - Google Patents
Verwendung von Reinaluminium für AluminiumdosenInfo
- Publication number
- DE2737232B2 DE2737232B2 DE2737232A DE2737232A DE2737232B2 DE 2737232 B2 DE2737232 B2 DE 2737232B2 DE 2737232 A DE2737232 A DE 2737232A DE 2737232 A DE2737232 A DE 2737232A DE 2737232 B2 DE2737232 B2 DE 2737232B2
- Authority
- DE
- Germany
- Prior art keywords
- aluminum
- pure aluminum
- cans
- pure
- zirconium
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Description
Die Erfindung betrifft die Verwendung von Reinaluminium für Aluminiumdosen mit einbrennlackiertem
Dosenkörper aus geglühten Leichtmetallbutzen.
Bekanntlich haben Weichglühbedingungen einen großen Einfluß auf das Entfestigungsverhalten gewalzter
Bleche bzw. fließgepreßter Dosenkörper. Letztere werden einbrenrhckiert, wobei durch Erholung ein
Anteil der Kaltverfestigung verloren geht.
Der in Rede stehenden Erfindung liegt der Gedanke zugrunde, mittels Zusätzen an piiritektischen Elementen
die Entfestigung beim Einbrennlackieren zu verhindern
bzw. gegenüber »reinem« Reinaluminium auf ein Minimum zu reduzieren. Das Einbrennlackieren wird
üblicherweise bei Temperaturen durchgeführt, die sicher unterhalb 25O°C liegen. Übliche Einbrennlacke
werden normalerweise bei Temperaturen um 2000C
verarbeitet
Hierzu stellt D. Altenpohl in »Aluminium und Aluminiumlegierungen«, 1965, auf Seite 344 ein
Temperatur/Glühzeit-Diagramm für Reinaluminium vor. Daraus läßt sich für eine Temperatur von 2500C
eine Zeit von 10 000 min. bis zur vollständigen primären Rekristallisation ablesen.
Bei der erfindungsgemäßen Verwendung von Reinaluminium
mit 0,05 bis 0,1% Silizium und 0,1 bis 0,25% Eisen für die Herstellung fließgepreßter und einbrennlackierter
Aluminiumdosen werden dem Reinaluminium zumindest zwei rekristallisationshemmende, sich in
Aluminium peritektisch verhaltende Elemente von jeweils 0,05 bis 0,3% zugattiert oder aber 0,05 bis 0,9%
Mangan.
Nach einem weiteren Merkmal hat es sich für den erstgenannten Fall als günstig erwiesen, daß weniger als
jeweils 0,2% Chrom und/oder Zirkonium und/oder jeweils 0,05 bis 0,20% Titan und Zirkonium zugattiert
werden.
Die von der Kaltverformung, i. e. Fließpressen, stammende Festigkeit soll nach der Lackeinbrennung
möglichst wenig abfallen und der Umformwiderstand durch rekristallisationshemmende Zusätze nicht erhöht
werden. So werden dem Reinaluminium mit beispielsweise 0,05 bis 0,1% Silizium und OJ bis 0,25% Eisen vor
seiner Verformung zumindest zwei rekristalliiationshemmende, sich in Aluminium peritektisch verhaltende
Elemente von jeweils 0,05 bis 0,3%, bevorzugtermaßen
weniger als jeweils 0,2% Chrom und/oder Titan und/oder Zirkonium zugattiert
Diese kleinen Zusatzmengen rekristallisationshemmender
Elemente verursachen eine Verminderung des Festigkeitsrückganges der kaltverfestigten Dosenkörper
beim Lackeinbrennen; diese Elemente müssen so dosiert sein, daß sie den Fließpreßvorgang nicht stören.
to Sowohl das Vergießen über Rotary und das Warmund Kaltwalzen als auch die übliche Butzenglühung
können beibehalten werden, was Investitionskosten vermeidet Ebenfalls ist es möglich, die Fertigung über
Butzen aus stranggepreßten Bändern durchzuführen.
υ In Versuchen wurden Reinaluminium-Butzen aus einem Warmwalzband einerseits und Reinaluminium-Butzen
mit Zusätzen von jeweils 0,1% Titan und. Zirkonium anderseits verglichen. Dosenkörper nach
einer dem Lackeinbrennen entsprechenden Wärmebehandlung aus erfindungsgemäß verwendeten Reinaluminium
weisen gegenüber den Dosen aus bisher üblichen Reinaiuminium-Butzen eine etwa 20% höhere
Zugfestigkeit auf. Die Materialeinsparung bei durch die erfindungsgemäße Verwendung hergestellten Dosen-
r, körpern beträgt etwa acht Prozent.
Weitere Vorteile der erfindungsgemäßen Verwendung ergeben sich aus der nachfolgender! Beschreibung
von Versuchsergebnissen sowie anhand der Zeichnung, welche eine graphische Gegenüberstellung von vier
«ι verschiedenen Versuchsresultaten wiedergibt.
Es wurden gemäß der folgenden Tabelle Butzen aus Blech von etwa 7 mm Dicke verschiedener Zusammensetzung
hergestellt und nach einer Aufheizzeit von ca. 40 Minuten in einem Luftumwälzofen etwa zehn
π Stunden lang bei 490° C geglüht.
Werk | Si | Fe | Ti | Cr | Zr |
stoff Nr. | % | % | /ο | % | % |
I | 0,09 | 0,25 | 0,02 | _ | _ |
II | 0,08 | 0,25 | 0,02 | - | 0,13 |
HI | 0,09 | 0,245 | 0,02 | 0,11 | 0,09 |
IV | 0,09 | 0,245 | 0,092 | - | 0,09 |
Anschließend wurden die Butzen zur Simulation des Fließpreßvorganges auf 0,5 mm kaltgewalzt sowie statt
des Einbrennvorganges bei 260°C im Salzbad geglüht und in Wasser abgeschreckt.
Bei dem in der Zeichnung dargestellten Koordinatensystem
ist auf der horizontalen Achse die Glühdauer für den simulierten Einbrennvorgang in Minuten angegeben;
die vertikale Achse gibt die Zugfestigkeit in kp/mm2an.
Vergleicht man nun die aufgetragenen Kurven zu den Materialzusammensetzungen I, II, III und IV, so wird
deutlich, um wieviel höher die Zugfestigkeit der mit Titan und Zirkonium gattierten Werkstoffe ist; so
beträgt der Unterschied der Zugfestigkeit nach einer Glühdauer von acht Minuten etwa 4 kp/mm2.
Die Festigkeitswerte von Dosenkörpern liegen etwas über den dargestellten Festigkeitswerten der Bleche;
die entsprechenden Kurven für Dosenkörper sind also parallel aufwärts verschoben.
liier/u I Blatt
Claims (4)
1. Verwendung von Reinaluminium mit 0,05 bis 0,1% Siiizium und 0,1 bis 0,25% Eisen für die
Herstellung fließgepreßter und einbrennlackierter Aluminiumdosen, wobei dem Reinaluminium zumindest
zwei rekristallisationshemmende, sich in Aluminium peritektisch verhaltende Elemente von jeweils
0,05 bis 0,3% zugattiert werden.
2. Verwendung von Reinaluminium mit 0,05 bis 0,1% Silizium und 0,1 bis 0,25% Eisen für die
Herstellung fließgepreBter und etnbrennlackierter
Aluminiumdosen, wobei dem Reinaluminium 0,05 bis 0,9% Mangan zugattiert werden.
3. Verwendung nach Anspruch I1 dadurch
gekennzeichnet, daß weniger als jeweils 0,2% Chrom und/oder Zirkonium zugattiert werden.
4. Verwendung nach Anspruch 1 oder 3, dadurch gekennzeichnet, daß jeweils 0,05 bis 0,20% Titan und
Zirkonium tugattiert werden.