CN110331531A - A kind of postfinishing process of frivolous blended suitable hair fancy suiting product - Google Patents

A kind of postfinishing process of frivolous blended suitable hair fancy suiting product Download PDF

Info

Publication number
CN110331531A
CN110331531A CN201910737445.0A CN201910737445A CN110331531A CN 110331531 A CN110331531 A CN 110331531A CN 201910737445 A CN201910737445 A CN 201910737445A CN 110331531 A CN110331531 A CN 110331531A
Authority
CN
China
Prior art keywords
fabric
pressure
steaming
postfinishing process
speed
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201910737445.0A
Other languages
Chinese (zh)
Other versions
CN110331531B (en
Inventor
孔斌斌
陈队范
陈建召
赵会堂
殷贺
姜卫坤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHANDONG COMPANION GROUP CO Ltd
Original Assignee
SHANDONG COMPANION GROUP CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHANDONG COMPANION GROUP CO Ltd filed Critical SHANDONG COMPANION GROUP CO Ltd
Publication of CN110331531A publication Critical patent/CN110331531A/en
Application granted granted Critical
Publication of CN110331531B publication Critical patent/CN110331531B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of postfinishing process of frivolous blended suitable hair fancy suiting product, include the following steps: S1: fabric is carried out to air-flow absorption washing in collator;S2: fulling processing;S3: open width is soft;S4: light steaming-fluffing-steaming-fluffing again;S5: wet brush;S6: hot light, cropping;S7: tank steams.The faults problem such as fabric folding line, shrink mark, abrasion, broken hole is effectively prevented by the method for the invention, and top-quality product rate is significantly promoted, and hundred meters of knot pigtail numbers are greatly lowered, and ensure that product quality.

Description

A kind of postfinishing process of frivolous blended suitable hair fancy suiting product
Technical field
The present invention relates to wool spinning final finishing technical fields, and in particular to a kind of final finishing of frivolous blended suitable hair fancy suiting product Technique.
Background technique
Frivolous blended suitable hair fancy suiting is fabric indispensable in high-grade dress ornament production, no matter from appearance and modeling or taking Highly recognition both domestic and external is all obtained in property.Current frivolous blended suitable hair fancy suiting generally by wool and silkworm silk blend and At in order to improve the gloss and pliability of fabric, it is therefore desirable to add the mulberry silk of larger proportion.Due to frivolous blended suitable hair flower Itself fabric is frivolous and the addition of mulberry silk larger proportion, makes frivolous blended suitable hair fancy suiting in afterfinish easily There are the faults such as shrink mark, folding line, abrasion, broken hole, brings many troublesome and inconvenience to arrangement process, influence product quality.
Also there are many professional class technical staff to improve entire production technology at present, but effect is unobvious.Therefore it mentions It is a technical problem to be solved urgently for a kind of postfinishing process for avoiding the faults such as fabric folding line, shrink mark, abrasion, broken hole.
Summary of the invention
In view of the above shortcomings of the prior art, the object of the present invention is to provide after a kind of frivolous blended suitable hair fancy suiting product Finishing technique.
To achieve the above object, the present invention adopts the following technical scheme:
The first aspect of the present invention provides a kind of postfinishing process of frivolous blended suitable hair fancy suiting product, including walks as follows It is rapid:
S1: fabric is carried out to air-flow absorption washing in collator;
S2: fulling processing;
S3: open width is soft;
S4: light steaming-fluffing-steaming-fluffing again;
S5: wet brush;
S6: hot light, cropping;
S7: tank steams.
The advanced promoting the circulation of qi stream absorption washing of final finishing step of the present invention, then fulling processing is carried out, open width softness is carried out after fulling, Decatizing is fluffed after softness, straight, the hot light cropping again after wet brush of wet brush after fluffing, is finally carried out tank and is steamed sizing.Through the above steps Sequential processes, fabric can be made gradually soft, gradually smooth, avoid fabric folding line, shrink mark, abrasion, broken hole etc. well The generation of fault, can make cloth cover it is smooth, without folding line, soft, while improving the top-quality product rate of product.
Preferably, the textile in step S1 includes: wool 40%-45%, mulberry silk 55%- by mass percentage 60%.Above-mentioned raw materials are woven into fabric, fabric weight 328-332g/m by conventional blended mode.
Preferably, the air-flow absorption washing in step S1 is to be placed on fabric to arrange on machine cylinder, by roller Negative pressure gas flow replaces mechanical pressure to adsorb fabric, is then finally sprayed by the lotion and water injection of atomization in fabric surface Jetting cleans lower machine;Wherein water temperature is 40-50 DEG C, and the fabric speed of service is 500-600m/min when cleaning, and wash time is 25min, the amount of lotion are the 3%-4% of fabric quality, and amount of water is 15-20 times of fabric quality, and fabric is transported when cleaning lower machine Scanning frequency degree is 200-300m/min.The collator is the CM101-350 type Multifunctional whole of Taian Companion Machinery Co., Ltd. Reason machine (air-flow is washed), fabric is less prone to crease in washing process not by action of mechanical pressure, while fabric can be made to become soft It is soft.The lotion uses the Efficient detergent of Beijing Zhong Fang Chemical Co., Ltd..
Preferably, in step s 2, fulling processing is the milling agent that fabric quality 6%-8% is added in gatte rwalking, is led to Cross the pressure roller of gatte rwalking, pressing plate squeezes fabric;Wherein the pressure of pressure roller and pressing plate is 0.01Mpa-0.03Mpa, contracting Temperature is 40 DEG C -45 DEG C, humidity 70%-80%, time 45min-50min.The milling agent uses in Beijing and spins chemical industry The milling agent of Co., Ltd model FK616.
Fulling processing can reduce the shrink mark that fulling is glued and formed using the slow contracting of light pressure.Have after air-flow absorption carrying out washing treatment It is broken to twist effect, rear feel soft fluffy is washed, during fulling, after milling agent is added, is bubbled immediately, it is maximum in terms of these Mitigate to limit wash, contracting folding line.The fulling time is reduced, 50min or so is down to by original 70min, therefore reduce fabric Occurs the probability of the faults such as broken hole, abrasion during fulling.
Preferably, in step S3, open width softness is fabric quality 3%-4% is separately added into before and after squezzing trough soft Soft dose, apply the pressure of 1100-1300Mpa, fabric speed of service speed 8-10m/min to fabric by water calender squeegee. Open width softness flattens cloth cover gauffer folding line, and cloth cover can also adsorb certain softening agent, enhances cloth surface evenness, without folding line, hand Sense is soft.The softening agent is the softening agent of Xintai City Dong great Zhi Jie Fine Chemical Co., Ltd model D2-B.
Preferably, in step S4, gently steaming and steam again is that fabric is put into decator to carry out decatizing, wherein the packet gently steamed Cloth pressure is 0.3Mpa-0.5Mpa;The infantees pressure steamed again is 0.3Mpa-0.5Mpa, platen pressure 0.2Mpa-0.4Mpa; Being fluffed twice using the specification of fluffing card clothing is 32 bugle needles, and is fluffed with single cylinder raising machine, fluffing 3-4 times every time.
Light steam only applies pressure to fabric by infantees, steams again and not only applies pressure to fabric by infantees, also passes through pressure Roller applies pressure to fabric.
To remove folding line, first decatizing is fluffed again, since product is frivolous, prevents the overstocked hair of extremely turning up of fabric irregular, therefore into Row steams again, solves to fluff again steam again after because of the problems such as folding line, item of fabric too small property life print, fluffing is uneven by steaming again, fluffing Afterwards fabrics cloth cover it is smooth without folding, soft have body bone.
Preferably, in step S5, the wet swiped through journey fabric speed of service is 8-10m/min, and be formed 12h.It is wet to be brushed with 6 bristle brush With 2 steel brushes, realize that product is more straight by wet brush, size is more stable.
Preferably, in step S6, the boiling hot roll temperature of hot light is 200-220 DEG C, and the fabric speed of service is 8-10m/min, is adjusted Whole hot light gauge is 5.2cm-5.5cm;
Cropping 3-4 times, the fabric speed of service is 6-8m/min when cropping, carries out a hot light before each cropping.
Since fabric is frivolous, hot light gauge is adjusted in hot light, prevent from giving a discount.Because of this product containing mulberry silk and Frivolous, cropping is easily skidded, and roll setting too great Yi goes out washboard print, therefore by increasing cropping number, makes cropping gauge slow play, and knit The object speed of service is also slow.
Preferably, tank steaming is put into fabric in tank steaming machine, and it is 95-100 DEG C that tank, which steams the temperature in machine steaming pot, and tank steams machine and adopts Fabric is rolled in interlayer with infantees, then passes through high-temperature steam, steam pressure 0.3Mpa-0.4Mpa, vapor (steam) temperature 150- 160 DEG C, tank steams 20-25min.
The tank steams machine and steams machine using Italy's TMT tank, is steamed by tank and carries out high temperature and pressure sizing to fabric, obtains preferable Fixed effect, promote fabric feeling, gloss, elasticity, make its dimensional stability, and the smooth no folding of cloth cover.
The second aspect of the present invention provides a kind of frivolous blended suitable hair fancy suiting product, is prepared by above-mentioned postfinishing process It forms.
Beneficial effects of the present invention:
(1) since frivolous blended suitable hair tweed fabric is frivolous, mulberry silk ratio is high, after being carried out by the method for the invention to it It arranges, can be good at the faults such as fabric folding line, shrink mark, abrasion, broken hole caused by solving because of above-mentioned factor, process stabilizing.
(2) present invention avoids fabric by mechanical pressure, in washing process not by air-flow absorption washing in washing process Easily there is crease, while fabric can be made to become soft.
(3) fulling processing can reduce the shrink mark that fulling is glued and formed using the slow contracting of light pressure.After air-flow adsorbs carrying out washing treatment There is broken twirl effect, wash rear feel soft fluffy, during fulling, after milling agent is added, is bubbled immediately, in terms of these most Mitigate to limits wash, contracting folding line;The fulling time is reduced, 50min or so is down to by original 70min, therefore reduce and knit There is the probability of the faults such as broken hole, abrasion during fulling in object.
It (4) is removal folding line, first decatizing is fluffed again, since product is frivolous, prevents the overstocked hair of extremely turning up of fabric irregular, therefore It is steamed again, by steaming the problems such as solving because of the raw folding line of fabric too small property, item print, fluffing unevenness again, fluffs, rise again steam again after After hair fabrics cloth cover it is smooth without folding, soft have body bone.
(5) since fabric is frivolous, hot light gauge is adjusted in hot light, prevent from giving a discount;Because this product contains silkworm Silk and it is frivolous, cropping is easily skidded, roll setting too great Yi go out washboard print, therefore by increase cropping number, make cropping gauge slow play, and And the fabric speed of service is also slow.
(6) by the cooperation of each step, the frivolous blended suitable hair fancy suiting after making final finishing is first-class without folding line, shrink mark Product rate increases substantially, and top-quality product rate is promoted to 97% or more by 70% or so, and hundred meters of knot pigtail numbers are down to 1.5 by 4.6 or so It is a or so, it ensure that product quality.
Specific embodiment
It is noted that following detailed description is all illustrative, it is intended to provide further instruction to the application.Unless another It indicates, all technical and scientific terms used herein has usual with the application person of an ordinary skill in the technical field The identical meanings of understanding.
In order to enable those skilled in the art can clearly understand the technical solution of the application, below with reference to tool The technical solution of the application is described in detail in the embodiment of body.
Embodiment 1
A kind of postfinishing process of frivolous blended suitable hair fancy suiting product, includes the following steps:
S1: fabric is carried out to air-flow absorption washing in collator: fabric being placed on and is arranged on machine cylinder, roller is passed through Interior negative pressure gas flow replaces mechanical pressure to adsorb fabric, then by the lotion and water injection of atomization in fabric surface, most Injection water cleans lower machine afterwards;Wherein water temperature is 40 DEG C, and the fabric speed of service is 500m/min, wash time 25min when cleaning, The amount of lotion is the 3% of fabric quality, and amount of water is 15 times of fabric quality, and the fabric speed of service is 200m/ when cleaning lower machine min.The collator is the CM101-350 type Multifunctional finishing machine (air-flow is washed) of Taian Companion Machinery Co., Ltd..Fabric Raw material includes: wool 40%, mulberry silk 60% by mass percentage.Above-mentioned raw materials are woven into fabric by conventional blended mode, Fabric weight is 328-332g/m.
S2: fulling processing: the milling agent of fabric quality 6% is added in gatte rwalking, passes through the pressure roller of gatte rwalking, pressing plate pair Fabric is squeezed;Wherein the pressure of pressure roller and pressing plate is 0.03Mpa, and fulling temperature is 40 DEG C, humidity 70%, and the time is 50min。
S3: open width is soft: being separately added into the softening agent of fabric quality 3% before and after squezzing trough, passes through water calender rubber Roller applies the pressure of 1300Mpa, fabric speed of service speed 3m/min to fabric.
S4: light steaming-fluffing-steaming-fluffing again: it is light steam and steam again be fabric is put into decator to carry out decatizing, wherein The infantees pressure gently steamed is 0.3Mpa;The infantees pressure steamed again is 0.3Mpa, platen pressure 0.4Mpa;Fluffing uses twice The specification of hair needle cloth is 32 bugle needles, and is fluffed with single cylinder raising machine, fluffing 3 times every time;
S5: wet brush: the fabric speed of service is 8m/min, and be formed 12h.It is wet to be brushed with 6 bristle brush and 2 steel brushes.
S6: hot light, cropping: the boiling hot roll temperature of hot light is 200 DEG C, and the fabric speed of service is 8m/min, adjusts hot light gauge For 5.2cm;Cropping 3 times, the fabric speed of service is 6m/min when cropping, carries out a hot light before each cropping.
S7: tank steams: fabric being put into Italian TMT tank steaming machine, it is 95 DEG C that tank, which steams the temperature in machine steaming pot, and tank steams machine and adopts Fabric is rolled in interlayer with infantees, then by high-temperature steam, steam pressure 0.3Mpa, vapor (steam) temperature is 160 DEG C, and tank steams 20min。
Embodiment 2
A kind of postfinishing process of frivolous blended suitable hair fancy suiting product, includes the following steps:
S1: fabric is carried out to air-flow absorption washing in collator: fabric being placed on and is arranged on machine cylinder, roller is passed through Interior negative pressure gas flow replaces mechanical pressure to adsorb fabric, then by the lotion and water injection of atomization in fabric surface, most Injection water cleans lower machine afterwards;Wherein water temperature is 50 DEG C, and the fabric speed of service is 600m/min, wash time 25min when cleaning, The amount of lotion is the 4% of fabric quality, and amount of water is 20 times of fabric quality, and the fabric speed of service is 300m/ when cleaning lower machine min.The collator is the CM101-350 type Multifunctional finishing machine (air-flow is washed) of Taian Companion Machinery Co., Ltd..Fabric Raw material includes: wool 45%, mulberry silk 55% by mass percentage.Above-mentioned raw materials are woven into fabric by conventional blended mode, Fabric weight is 328-332g/m.
S2: fulling processing: the milling agent of fabric quality 8% is added in gatte rwalking, passes through the pressure roller of gatte rwalking, pressing plate pair Fabric is squeezed;Wherein the pressure of pressure roller and pressing plate is 0.01Mpa, and fulling temperature is 45 DEG C, humidity 80%, and the time is 45min。
S3: open width is soft: being separately added into the softening agent of fabric quality 4% before and after squezzing trough, passes through water calender rubber Roller applies the pressure of 1100Mpa, fabric speed of service speed 6m/min to fabric.
S4: light steaming-fluffing-steaming-fluffing again: it is light steam and steam again be fabric is put into decator to carry out decatizing, wherein The infantees pressure gently steamed is 0.5Mpa;The infantees pressure steamed again is 0.5Mpa, platen pressure 0.2Mpa;Fluffing uses twice The specification of hair needle cloth is 32 bugle needles, and is fluffed with single cylinder raising machine, fluffing 4 times every time;
S5: wet brush: the fabric speed of service is 10m/min, and be formed 12h.It is wet to be brushed with 6 bristle brush and 2 steel brushes.
S6: hot light, cropping: the boiling hot roll temperature of hot light is 220 DEG C, and the fabric speed of service is 10m/min, adjusts hot light gauge For 5.5cm;Cropping 4 times, the fabric speed of service is 8m/min when cropping, carries out a hot light before each cropping.
S7: tank steams: fabric being put into Italian TMT tank steaming machine, it is 100 DEG C that tank, which steams the temperature in machine steaming pot, and tank steams machine Fabric is rolled in interlayer using infantees, then by high-temperature steam, steam pressure 0.4Mpa, vapor (steam) temperature is 150 DEG C, and tank steams 25min。
Embodiment 3
A kind of postfinishing process of frivolous blended suitable hair fancy suiting product, includes the following steps:
S1: fabric is carried out to air-flow absorption washing in collator: fabric being placed on and is arranged on machine cylinder, roller is passed through Interior negative pressure gas flow replaces mechanical pressure to adsorb fabric, then by the lotion and water injection of atomization in fabric surface, most Injection water cleans lower machine afterwards;Wherein water temperature is 45 DEG C, and the fabric speed of service is 550m/min, wash time 25min when cleaning, The amount of lotion is the 3% of fabric quality, and amount of water is 18 times of fabric quality, and the fabric speed of service is 260m/ when cleaning lower machine min.The collator is the CM101-350 type Multifunctional finishing machine (air-flow is washed) of Taian Companion Machinery Co., Ltd..Fabric Raw material includes: wool 43%, mulberry silk 57% by mass percentage.Above-mentioned raw materials are woven into fabric by conventional blended mode, Fabric weight is 328-332g/m.
S2: fulling processing: the milling agent of fabric quality 7% is added in gatte rwalking, passes through the pressure roller of gatte rwalking, pressing plate pair Fabric is squeezed;Wherein the pressure of pressure roller and pressing plate is 0.02Mpa, and fulling temperature is 43 DEG C, humidity 75%, and the time is 48min。
S3: open width is soft: being separately added into the softening agent of fabric quality 3% before and after squezzing trough, passes through water calender rubber Roller applies the pressure of 1200Mpa, fabric speed of service speed 5m/min to fabric.
S4: light steaming-fluffing-steaming-fluffing again: it is light steam and steam again be fabric is put into decator to carry out decatizing, wherein The infantees pressure gently steamed is 0.4Mpa;The infantees pressure steamed again is 0.4Mpa, platen pressure 0.3Mpa;Fluffing uses twice The specification of hair needle cloth is 32 bugle needles, and is fluffed with single cylinder raising machine, fluffing 3 times every time;
S5: wet brush: the fabric speed of service is 9m/min, and be formed 12h.It is wet to be brushed with 6 bristle brush and 2 steel brushes.
S6: hot light, cropping: the boiling hot roll temperature of hot light is 210 DEG C, and the fabric speed of service is 9m/min, adjusts hot light gauge For 5.3cm;Cropping 4 times, the fabric speed of service is 7m/min when cropping, carries out a hot light before each cropping.
S7: tank steams: fabric being put into Italian TMT tank steaming machine, it is 98 DEG C that tank, which steams the temperature in machine steaming pot, and tank steams machine and adopts Fabric is rolled in interlayer with infantees, then by high-temperature steam, steam pressure 0.3Mpa, vapor (steam) temperature is 155 DEG C, and tank steams 25min。
Product quality detection
Frivolous blended suitable hair fancy suiting made from above-described embodiment 1-3 is subjected to quality testing, top-quality product rate according to GB18401-2010 " national general safety technical code for textile products " is detected;Hundred meters of knot pigtail numbers are the items certain in breadth Under part, the number of 100 meters of knot pigtails;Testing result is as shown in the table:
Embodiment 1 Embodiment 2 Embodiment 3
Top-quality product rate (%) 97 97.1 97.8
Hundred meters of knot pigtail numbers (a) 1.6 1.5 1.3
As seen from the above table, the product produced by the method for the invention, top-quality product rate exist in 97% or more, hundred meter of knot pigtail number 1.5 or so, product quality is excellent, wherein the product quality of 3 method production is optimal through the embodiment of the present invention.
The foregoing is merely preferred embodiment of the present application, are not intended to limit this application, for the skill of this field For art personnel, various changes and changes are possible in this application.Within the spirit and principles of this application, made any to repair Change, equivalent replacement, improvement etc., should be included within the scope of protection of this application.

Claims (10)

1. a kind of postfinishing process of frivolous blended suitable hair fancy suiting product, which comprises the steps of:
S1: fabric is carried out to air-flow absorption washing in collator;
S2: fulling processing;
S3: open width is soft;
S4: light steaming-fluffing-steaming-fluffing again;
S5: wet brush;
S6: hot light, cropping;
S7: tank steams.
2. postfinishing process according to claim 1, which is characterized in that the textile in step S1 is by mass percentage It include: wool 40%-45%, mulberry silk 55%-60%.
3. postfinishing process according to claim 1, which is characterized in that the air-flow absorption washing in step S1 is by fabric It is placed on and arranges on machine cylinder, replace mechanical pressure to adsorb fabric by the negative pressure gas flow in roller, then pass through atomization Lotion and water injection in fabric surface, finally spray water and clean lower machine;Wherein water temperature is 40-50 DEG C, and fabric is run when cleaning Speed is 500-600m/min, and wash time 25min, the amount of lotion is the 3%-4% of fabric quality, and amount of water is fabric matter 15-20 times of amount, the flushing fabric speed of service are 200-300m/min.
4. postfinishing process according to claim 1, which is characterized in that in step s 2, fulling processing is in gatte rwalking The interior milling agent that fabric quality 6%-8% is added, squeezes fabric by the pressure roller of gatte rwalking, pressing plate;Wherein pressure roller and The pressure of pressing plate is 0.01Mpa-0.03Mpa, and fulling temperature is 40 DEG C -45 DEG C, humidity 70%-80%, time 45min- 50min。
5. postfinishing process according to claim 1, which is characterized in that in step S3, open width softness is in squezzing trough Front and back be separately added into the softening agent of fabric quality 3%-4%, 1100-1300Mpa is applied to fabric by water calender squeegee Pressure, fabric speed of service speed 8-10m/min.
6. postfinishing process according to claim 1 again, which is characterized in that in step S4, gently steaming and steam is by fabric It is put into decator and carries out decatizing, wherein the infantees pressure gently steamed is 0.3Mpa-0.5Mpa;The infantees pressure steamed again is 0.3Mpa-0.5Mpa, platen pressure 0.2Mpa-0.4Mpa;Being fluffed twice using the specification of fluffing card clothing is 32# needle cloth, And fluffed with single cylinder raising machine, fluffing 3-4 times every time.
7. postfinishing process according to claim 1, which is characterized in that in step S5, the wet swiped through journey fabric speed of service For 8-10m/min, be formed 12h.
8. postfinishing process according to claim 1, which is characterized in that in step S6, the boiling hot roll temperature of hot light is 200- 220 DEG C, the fabric speed of service is 8-10m/min, and adjustment hot light gauge is 5.2cm-5.5cm;
Cropping 3-4 times, the fabric speed of service is 6-8m/min when cropping, carries out a hot light before each cropping.
9. postfinishing process according to claim 1, which is characterized in that in step S7, tank steaming is that fabric is put into tank steaming In machine, it is 95-100 DEG C that tank, which steams the temperature in machine steaming pot, and tank is steamed machine and fabric is rolled in interlayer using infantees, then is steamed by high temperature Vapour, steam pressure 0.3Mpa-0.4Mpa, vapor (steam) temperature are 150-160 DEG C, and tank steams 20-25min.
10. a kind of frivolous blended suitable hair fancy suiting product, which is characterized in that by the described in any item rear finishing duplex of claim 1-9 Skill is prepared.
CN201910737445.0A 2019-06-19 2019-08-09 After-finishing process of light and thin blended smooth tweed product Active CN110331531B (en)