CN108728961A - A kind of cashmere water soluble fiber mixing spinning method for genuine - Google Patents
A kind of cashmere water soluble fiber mixing spinning method for genuine Download PDFInfo
- Publication number
- CN108728961A CN108728961A CN201810610269.XA CN201810610269A CN108728961A CN 108728961 A CN108728961 A CN 108728961A CN 201810610269 A CN201810610269 A CN 201810610269A CN 108728961 A CN108728961 A CN 108728961A
- Authority
- CN
- China
- Prior art keywords
- water soluble
- cashmere
- soluble fiber
- spinning method
- genuine
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Withdrawn
Abstract
The present invention relates to cashmere fiber mixing spinning technology fields, and in particular to a kind of cashmere water soluble fiber mixing spinning method for genuine.A kind of cashmere water soluble fiber mixing spinning method for genuine of the present invention, the technique twisted thread using conjunction hair-carding-grilling-combing-drafting-rove-spun yarn-automatic winding-doubling-.The present invention has at least one of following advantages and good effect:A kind of cashmere water soluble fiber mixing spinning method for genuine through the invention can produce the good cashmere water soluble fiber mixing weaving yarn of performance indicator by the way that cashmere, water soluble fiber is blended.After water soluble fiber dissolving, appearance of fabrics is plentiful, quality bulky, soft high Zhi Jingfang yarns, simple for process, of low cost, meets the demand in market, is with a wide range of applications in textile processing field.
Description
Technical field
The present invention relates to cashmere fiber mixing spinning technology fields, and in particular to a kind of cashmere water soluble fiber mixing spinning side
Method.
Background technology
With the continuous improvement of social progress and quality of life, requirement of the people to textile, not only fabric are protected
Warm, comfortably, and it is hoped that there will be more functions.
Cashmere is the bottom fine hair with goat, and caprine growth is on high and cold grassland, such as Chinese Inner Mongol, newly
The ground such as boundary, Qinghai, Liaoning.China is cashmere big producer in the world, and cashmere yield accounts for 70% of Gross World Product or more,
In especially using the cashmere of Inner Mongol as top grade.The characteristics of cashmere fiber, is very thin, soft, and fabric hand feel is soft, cunning is glutinous, gloss is soft,
Compared with the wool fabric of same thickness compared to it is light-weight very much, and mostly matte style, magnificent elegance.Especially cashmere has naturally
Turn bent, cohesive force is big, growth is big, water soluble fiber regularity is good, requires high, feature soluble easily in water to humiture.
In recent years, Chinese Cashmere Industry material outlet simple in is developed to suitable scientific and technological content and higher
The cashmere product exported country of added value.Pattern, the style of various cashmere products have extensive acclaim in the world.Since cashmere produces
Demand is huge in world markets for product, but cashmere resources are again very limited, thus cashmere is at high price.If developing mountain simply
The cultivation quantity of sheep, has an adverse effect to grassland ecology.In order to preserve the ecological environment, relevant departments take measures to limit goat
Cultivation quantity so that cashmere resources are relatively limited.In order to solve this contradiction, people attempt cashmere and other fabrics
It is blended.WATER-SOLUBLE PVA FIBER is a kind of functional differential fibers, it has the performance of common polyvinyl staple fiber, is added through special
Work modification can completely dissolve in water, have ideal water solution temperature, intensity and degree of stretching, have it is good it is acidproof, alkaline-resisting,
Dry heat resistance energy.WATER-SOLUBLE PVA FIBER is dissolved in tasteless nontoxic after water, and aqueous solution in a relatively short period of time can in colorless and transparent
Natural decomposition does not generate environment any pollution, is ideal environment-friendly products.
For this purpose, the application proposes a kind of cashmere water soluble fiber mixing spinning method for genuine, to solve the above problems.
Invention content
A primary object of the present invention is to overcome at least one defect in the prior art, provides a kind of production technology
Simply, low-cost cashmere water soluble fiber mixing spinning method for genuine.
In order to realize that above-mentioned technical proposal, the present invention use following technical scheme:
According to an aspect of the present invention, a kind of cashmere water soluble fiber mixing spinning method for genuine is provided, using conjunction hair-carding-
The technique that grilling-combing-drafting-rove-spun yarn-automatic winding-doubling-is twisted thread;Wherein,
Close hair:Cashmere, water soluble fiber are fed intake, after addition and crude oil, electrostatic agent and bleeding agent, the health in hair bonding bin
8~12 hours, make grease fully penetrated, then mix by mixing willow shredding;
Carding:The technological principle that combing machine for fur uses light quantitative, low velocity, comb more is to improve mixture homogeneity;Wherein, raw
Item quantification of 3g/5m, cylinder speed 320r/min, doffer speed 20r/min, licker-in speed 900r/min, cylinder-lid
Plate gauge is 17mm, 15mm, 13mm, 12mm, and cylinder-doffer's gauge is 5mm;
Grilling:Gill box uses drafting multiple for 3 times, the technological principle of close setting 25mm, slow train speed;
Combing:Combing machine uses the technological principle for removing short flannel, impurity of close setting 26mm, light quantitative, more radical 24;
Drafting:Drawing frame slowed down using speed, big gauge of pressurizeing again, gently quantitative technological principle, with cashmere and water-soluble fibre
It is mixed to tie up strip item;Wherein, roller gauge is 10mm × 16mm, and drafting multiple is 6 times, and loudspeaker are φ 3.2mm, Hardness 85
Degree;
Rove:Fly frame is using slow train speed, again pressurization, light quantitative, small tension receiving coil technological principle;Wherein, roving twist is
45, total draft is 7.2 times, and back area draft is 1.276 times, and roller gauge is 20mm × 34mm, ingot speed 615r/min;
Spun yarn:Spinning frame using small drawing-off, middle gauge, middle drawing-off, the big twist, slow train speed technological principle;Wherein, spun yarn
The twist is 900, and roller gauge is 21mm × 40mm, and back area draft is 1.346 times, ingot speed 6000r/min;
Automatic winding:In winding process, removal yarn is caused by tension, thickness section, evenness fault factor controlling are improper
Broken end, yarn defect;
Doubling:By several single-strand yarns and it is integrated;
It twists thread:The above-mentioned yarn to merge into a single whole is twisted one, obtains cashmere water soluble fiber finished product.
According to an embodiment of the present invention, the parts by weight of the cashmere are 70 parts by weight, the weight of the water soluble fiber
Part is 30 parts by weight.
According to an embodiment of the present invention, after being mixed by mixing willow shredding, the cashmere, water soluble fiber moisture regain control
System is 20%~23%, and at 25 DEG C, relative humidity is controlled 65%~75% for workshop temperature control.
According to an embodiment of the present invention, the fusing point of the water soluble fiber strip is 90 DEG C.
According to an embodiment of the present invention, the technological process of the grilling includes:The needle of scalp acupuncture (silver mixing vsn) → tri- (reason
Vsn) → bis- needle (manage bar vsn).
According to an embodiment of the present invention, the technological process of the combing includes:The needle of multiple scalp acupuncture (silver mixing vsn) → tetra-
(neat and well spaced vsn) → multiple four needles (neat and well spaced vsn) → bis- needle (manage bar vsn).
In the present invention, through cashmere described in many experiments and water soluble fiber using mixed mixing method is dissipated, after water-break is molten, have
The advantages that item is dry uniformly, yarn count fault is few.
As shown from the above technical solution, the present invention has at least one of following advantages and good effect:
A kind of cashmere water soluble fiber mixing spinning method for genuine through the invention, passes through blended, the energy by cashmere, water soluble fiber
Enough produce the good cashmere water soluble fiber mixing weaving yarn of performance indicator.After water soluble fiber dissolving, appearance of fabrics is plentiful, quality pine
Thickness, soft high Zhi Jingfang yarns are simple for process, of low cost, the demand in market met, in textile processing field
It is with a wide range of applications.
Description of the drawings
Fig. 1 is the process flow chart of cashmere water soluble fiber mixing spinning method for genuine of the present invention.
Specific implementation mode
In the description of the present invention, unless otherwise indicated, the meaning of " plurality " is two or more.Term "inner",
The orientation or state relation of the instructions such as "upper", "lower" are orientation based on ... shown in the drawings or state relation, are merely for convenience of retouching
It states the present invention and simplifies description, do not indicate or imply the indicated device or element must have a particular orientation, with specific
Azimuth configuration and operation, therefore be not considered as limiting the invention.
In the description of the present invention, it should be noted that unless otherwise clearly defined and limited, term " installation " " connects
Connect " it shall be understood in a broad sense, for example, it may be being fixedly connected, it may be a detachable connection, or be integrally connected;It can be machine
Tool connects, and can also be electrical connection;It can be directly connected, it can also be indirectly connected through an intermediary.For this field
For those of ordinary skill, the concrete meaning of above-mentioned term in the present invention is understood as the case may be.
Below in conjunction with the accompanying drawings and specific implementation mode invention is further described in detail.
Referring to Fig. 1, Fig. 1 is the process flow chart of cashmere water soluble fiber mixing spinning method for genuine of the present invention.
A kind of cashmere water soluble fiber mixing spinning method for genuine of the present invention, using conjunction hair-carding-grilling-combing-drafting-
The processing step that rove-spun yarn-automatic winding-doubling-is twisted thread.
In the present invention, in the conjunction hair step, cashmere, water soluble fiber are fed intake, the parts by weight of the cashmere are 70 weight
Part, the parts by weight of the water soluble fiber are 30 parts by weight.After addition and crude oil, electrostatic agent and bleeding agent, supported in hair bonding bin
It is 8~12 hours raw, make grease fully penetrated, then mix by mixing willow shredding;After being mixed by mixing willow shredding, the sheep
Suede, water soluble fiber moisture regain control are 20%~23%, and at 25 DEG C, relative humidity is controlled 65%~75% for workshop temperature control.
In the present invention, in the carding step, since water soluble fiber is without natural convolution, obvolvent force difference, elongation is small, is processing
More difficulty is shifted in the process, and broken hole phenomenon easily occurs in fleece, therefore weight of card sliver should be appropriate less than normal, cylinder speed and licker-in speed
Degree should be reduced suitably to reduce short fiber content.Therefore in production, combing machine for fur is using light quantitative, low velocity, the technological principle more combed
To improve mixture homogeneity.Wherein, weight of card sliver 3g/5m, cylinder speed 320r/min, doffer speed 20r/min, thorn
Roller speed is 900r/min, and cylinder-Flat Gauge is 17mm, 15mm, 13mm, 12mm, and cylinder-doffer's gauge is 5mm.
In the present invention, in the grilling step, gill box uses drafting multiple for 3 times, the work of close setting 25mm, slow train speed
Skill principle.Wherein, the concrete technology flow process of the grilling includes:Needle (the reason of the needle (manage bar vsn) of scalp acupuncture (silver mixing vsn) → tri- → bis-
Vsn), it is specific as follows:
Scalp acupuncture:Feeding radical 10, gauge 25mm, 2.86 times of drawing-off, item weigh 17 ± 1g, 5 needle of needle number, speed 18%, are
Keep item dry uniform, using more radicals, close setting, small drawing-off, slow train speed;
Three needles:Feeding radical 2, gauge 25mm, 2.86 times of drawing-off, item weigh 12 ± 1g, needle number 6, speed 18%;
Two needles:Feeding radical 2 × 2, gauge 25mm, 2.86 times of drawing-off, item weigh 8 ± 1g, 6 needle of needle number, speed 18%.
In the present invention, in the combing step, combing machine using close setting 26mm, light quantitative, more radical 24 go it is short
The technological principle of suede, impurity.Radical 24, gauge 26mm, drafting multiple 14 are fed, item weighs 12 ± 1g, and speed 200 clamps time/
Point.Wherein, the technological process of the combing includes:Answering scalp acupuncture (silver mixing vsn) → tetra- needles (neat and well spaced vsn) →, it is (neat and well spaced to answer four needles
Vsn) → bis- needle (manage bar vsn), it is specific as follows:
Multiple scalp acupuncture:Feeding radical 4, gauge 25mm, 2.86 times of drawing-off, item weigh 15 ± 1g, 5 needle of needle number, speed 18%;
Four needles:Feeding radical 6, gauge 25mm, 2.86 times of drawing-off, item weigh 15 ± 1g, speed 18%, 7 needle of needle number;
Multiple four needles:Feeding radical 5, gauge 25mm, 2.86 times of drawing-off, item weigh 15 ± 1g, speed 18%, 7 needle of needle number;
Multiple two needles:Feeding radical 2 × 2, gauge 25mm, 2.86 times of drawing-off, item weigh 8 ± 1g, 6 needle of needle number, speed 18%.
In the present invention, in the drafting step, drawing frame slowed down using speed, big gauge of pressurizeing again, gently quantitative technique
Principle, mixed with cashmere and water soluble fiber strip item, the fusing point of the water soluble fiber strip is 90 DEG C;Wherein, roller gauge is
10mm × 16mm, drafting multiple are 6 times, and loudspeaker are φ 3.2mm, and Hardness is 85 degree.
In the present invention, in the rove step, under the premise of spun yarn energy drawing-off can not open rubber yarn, rove when rove
The twist suitably bigger than normal, water soluble fiber obvolvent force difference, raising roving twist should slip problem when being avoided that spun yarn drafting.Fly frame is adopted
With slow train speed, again pressurization, light quantitative, small tension receiving coil technological principle.Wherein, roving twist 45, total draft are 7.2 times, back zone
Drawing-off is 1.276 times, and roller gauge is 20mm × 34mm, ingot speed 615r/min.
In the present invention, in the spun yarn step, since spun yarn end breakage rate is high, rubber yarn and filoplume are more, item does poor, drawing-off
Multiple grasp less than normal easily improves spinning evenness, and the twist is bigger than normal to be avoided that the problems such as strength is low, broken end is more caused by spun yarn slips.
Spinning frame using small drawing-off, middle gauge, middle drawing-off, the big twist, slow train speed technological principle;Wherein, ramie yarn twist 900, sieve
Drawing gauge is 21mm × 40mm, and back area draft is 1.346 times, ingot speed 6000r/min.
In the present invention, in the automatic winding, in winding process, removal yarn because tension, thickness section, evenness fault because
Broken end, yarn defect caused by element control is improper.In the doubling step, by several single-strand yarns and it is integrated.The step of twisting thread
In rapid, the above-mentioned yarn to merge into a single whole is twisted one, obtains cashmere water soluble fiber finished product.
Wherein, in the automatic winding and step of twisting thread, yarn is reduced because of tension, thickness section, evenness fault factor controlling
Broken end, yarn defect caused by improper.
In the present embodiment, the conjunction hair use BC262 mixing willows, the carding use FA201B combing machine for furs, it is described simultaneously
Strip adoption FA302 drawing frames, the rove use FA454 fly frames, the spun yarn to use FA506 spinning frames, the automatic network
Cylinder uses automatic winder 338, and the doubling uses FA705 doubling frames, described to twist thread using FA761 twisting machines.It needs to illustrate
, above equipment is existing equipment, and those skilled in the art can select different models according to actual demand.
A kind of cashmere water soluble fiber mixing spinning method for genuine through the invention, can produce a kind of 70 parts by weight of parts by weight
60 blended public affairs Zhi Jingfang hosiery yarns of cashmere, 30 parts by weight water soluble fibers.
In conclusion a kind of cashmere water soluble fiber mixing spinning method for genuine through the invention, by by cashmere, water-soluble fibre
It ties up blended, performance indicator good cashmere water soluble fiber mixing weaving yarn can be produced.After water soluble fiber dissolving, appearance of fabrics is rich
Full, quality bulky, soft high Zhi Jingfang yarns are simple for process, of low cost, meet the demand in market, weaving
It is with a wide range of applications in manufacture field.
Claims (6)
1. a kind of cashmere water soluble fiber mixing spinning method for genuine, which is characterized in that thick using hair-carding-grilling-combing-drafting-is closed
The technique that yarn-spun yarn-automatic winding-doubling-is twisted thread;Wherein,
Close hair:Cashmere, water soluble fiber are fed intake, after addition and crude oil, electrostatic agent and bleeding agent, in hair bonding bin health 8~
12 hours, make grease fully penetrated, then mix by mixing willow shredding;
Carding:The technological principle that combing machine for fur uses light quantitative, low velocity, comb more is to improve mixture homogeneity;Wherein, the carded sliver is fixed
Amount be 3g/5m, cylinder speed 320r/min, doffer speed 20r/min, licker-in speed 900r/min, cylinder-cover board every
Away from for 17mm, 15mm, 13mm, 12mm, cylinder-doffer's gauge is 5mm;
Grilling:Gill box uses drafting multiple for 3 times, the technological principle of close setting 25mm, slow train speed;
Combing:Combing machine uses the technological principle for removing short flannel, impurity of close setting 26mm, light quantitative, more radical 24;
Drafting:Drawing frame slowed down using speed, big gauge of pressurizeing again, gently quantitative technological principle, with cashmere and water soluble fiber item
Sub- item is mixed;Wherein, roller gauge is 10mm × 16mm, and drafting multiple is 6 times, and loudspeaker are φ 3.2mm, and Hardness is 85 degree;
Rove:Fly frame is using slow train speed, again pressurization, light quantitative, small tension receiving coil technological principle;Wherein, roving twist 45, always
Drawing-off is 7.2 times, and back area draft is 1.276 times, and roller gauge is 20mm × 34mm, ingot speed 615r/min;
Spun yarn:Spinning frame using small drawing-off, middle gauge, middle drawing-off, the big twist, slow train speed technological principle;Wherein, ramie yarn twist
It is 900, roller gauge is 21mm × 40mm, and back area draft is 1.346 times, ingot speed 6000r/min;
Automatic winding:In winding process, removal yarn breaks caused by tension, thickness section, evenness fault factor controlling are improper
Head, yarn defect;
Doubling:By several single-strand yarns and it is integrated;
It twists thread:The above-mentioned yarn to merge into a single whole is twisted one, obtains cashmere water soluble fiber finished product.
2. a kind of cashmere water soluble fiber mixing spinning method for genuine according to claim 1, which is characterized in that the weight of the cashmere
Amount part is 70 parts by weight, and the parts by weight of the water soluble fiber are 30 parts by weight.
3. a kind of cashmere water soluble fiber mixing spinning method for genuine according to claim 1, which is characterized in that passing through mixing willow
After shredding mixing, the cashmere, water soluble fiber moisture regain control are 20%~23%, and workshop temperature control is at 25 DEG C, relative humidity
Control is 65%~75%.
4. a kind of cashmere water soluble fiber mixing spinning method for genuine according to claim 1, which is characterized in that the water soluble fiber
The fusing point of strip is 90 DEG C.
5. a kind of cashmere water soluble fiber mixing spinning method for genuine according to claim 1, which is characterized in that the work of the grilling
Skill flow includes:The needle (manage bar vsn) of the needle (manage bar vsn) of scalp acupuncture (silver mixing vsn) → tri- → bis-.
6. a kind of cashmere water soluble fiber mixing spinning method for genuine according to claim 1, which is characterized in that the work of the combing
Skill flow includes:It answers scalp acupuncture (silver mixing vsn) → tetra- needles (neat and well spaced vsn) → and answers four needles (neat and well spaced vsn) → bis- needle (manage bar vsn).