CN106510007A - Production method of formaldehyde-free wash-and-wear shirt - Google Patents

Production method of formaldehyde-free wash-and-wear shirt Download PDF

Info

Publication number
CN106510007A
CN106510007A CN201611189960.2A CN201611189960A CN106510007A CN 106510007 A CN106510007 A CN 106510007A CN 201611189960 A CN201611189960 A CN 201611189960A CN 106510007 A CN106510007 A CN 106510007A
Authority
CN
China
Prior art keywords
formaldehyde
shirt
press finishing
free durable
finishing liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201611189960.2A
Other languages
Chinese (zh)
Inventor
陈丽芬
王洪明
赵维强
佘振云
陶瑞亮
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Sunshine Co Ltd
Original Assignee
Jiangsu Sunshine Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangsu Sunshine Co Ltd filed Critical Jiangsu Sunshine Co Ltd
Priority to CN201611189960.2A priority Critical patent/CN106510007A/en
Publication of CN106510007A publication Critical patent/CN106510007A/en
Priority to PCT/CN2017/083800 priority patent/WO2018113169A1/en
Pending legal-status Critical Current

Abstract

The invention relates to a production method of formaldehyde-free wash-and-wear shirt. The production method is characterized by sequentially comprising production steps of sewing the shirt, washing the shirt in water, drying the shirt, spraying formaldehyde-free non-ironing finishing liquid, pre-drying the skirt, pre-ironing the skirt, pressing the shirt, baking the skirt, freezing the shirt, washing the obtained shirt in water, drying the obtained shirt and packaging the obtained skirt, wherein by spraying the formaldehyde-free non-ironing finishing liquid, a liquid carrying rate of the skirt can reach 65-90% or above; the formaldehyde-free non-ironing finishing liquid consists of the following components: non-ironing resin, a fiber protective agent, a softening agent, a catalyst and water; the operation of pre-drying the skirt is conducted at 40-60 DEG C, and the liquid carrying rate of the skirt which is pre-dried can reach 20-50% or above; the operation of baking the skirt is conducted at 140-160 DEG C for 3-7min; and the operation of freezing the skirt is conducted at minus 10-0 DEG C for 0.5-1.5h, and the humidity of a freezing chamber is 60-90%. The production method provided by the invention has the advantages that the method, in a whole skirt production process, is free from the generation of formaldehyde, and the finished wash-and-wear skirt product is free from formaldehyde residue as well.

Description

A kind of production method of formaldehydeless wash-and-wear of shirt
Technical field
A kind of a kind of the present invention relates to production method of shirt, more particularly to production method of formaldehydeless wash-and-wear of shirt.
Background technology
At present the production craft step of wash-and-wear of shirt is followed successively by shirt sewing, washing, drying, sprinkling noniron finish liquid, pre- Baking, pressing, sizing, finished product washing, finished product drying and finished product packing, due to containing aldehyde radical in noniron finish liquid, so exempting from Formaldehyde can be produced in boiling hot shirt preparation process, production environment is impacted, and contain formaldehyde in causing finished product shirt, in people Harmful effect is produced to human body skin when body is worn.
The content of the invention
It is an object of the invention to provide a kind of production method of formaldehydeless wash-and-wear of shirt, its nothing in shirt production process Form aldehyde release, while do not contain formaldehyde in finished product wash-and-wear of shirt.
The present invention technology contents be, a kind of production method of formaldehydeless wash-and-wear of shirt, it is characterised in that production stage according to It is secondary for shirt sewing, washing, drying, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, product water Wash, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 65~90%, described formaldehyde-free durable-press finishing liquid Component is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, and no-ironing resin is in formaldehyde-free durable-press finishing liquid Concentration be 150~240g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid be 30~50g/ L, softening agent Concentration in formaldehyde-free durable-press finishing liquid be 20~60g/ L, concentration of the catalyst in formaldehyde-free durable-press finishing liquid be 15~ 35g/ L;
The temperature of preliminary drying is 40~60 DEG C, and after preliminary drying, the liquid carrying rate of shirt reaches 20~50%;
Bake as making no-ironing resin and fiber crosslink reaction, reach wrinkle resistant non-ironing effect, the temperature for baking for 140~ 160 DEG C, the time is 3~7 minutes;
Freezing is that the shirt after baking is put into refrigerating chamber freezing, and the temperature of freezing is 10~0 DEG C, cooling time is 0.5~ 1.5 hours, the humidity of refrigerating chamber was 60~90%, and the cellulose fibre of shirt is due to easily becoming under the hot environment for baking Out-of-flatness, surface easily play concavo-convex bubble, and as the temperature for freezing is relatively low, ambient humidity during freezing is of a relatively high, gives just The certain humidity of shirt that high temperature is baked so as to which regain is further improved so that the fracture of blouse fabric and tearing has been carried Height, can also make that ready-made clothes feel is more smooth in addition, and quick freeze can stop the reaction of dressing liquid, reply bafta moment flat It is whole, reach more preferable appearance.
In the production method of above-mentioned formaldehydeless wash-and-wear of shirt, in formaldehyde-free durable-press finishing liquid, no-ironing resin is Germany The Arkofix NZK of CLARIANT companies, the protorez ffo of tanatex companies of Holland, HUNTSMAN companies of the U.S. The Fixapret NF of KNITEX FF, the REACEL ZF of BOZZETTO companies of Italy or BASF Corp. of Germany;
Fiber protection agent is the Ceranine HDP. of German CLARIANT companies, the persoftal of tanatex companies of Holland The Perapret additive peb of pe25, the WELLIN PE of BOZZETTO companies of Italy or BASF Corp. of Germany;
Softening agent is the Solusoft MW or SE1 of German CLARIANT companies, the persoftal of tanatex companies of Holland Sme, the DICRYLAN WK of HUNTSMAN companies of the U.S., the SEBOSAN SNC of BOZZETTO companies of Italy or Germany BASF are public The Sliligen sih of department;
Catalyst is the Catalyst NKC of German CLARIANT companies, the KNITEX MO of HUNTSMAN companies of the U.S., Italy The CATAL MCA of the BOZZETTO companies or Fixapret f-m of BASF Corp. of Germany.
In the production method of above-mentioned formaldehydeless wash-and-wear of shirt, shirt sewing, washing, drying, pre- boiling hot, pressing, product water Wash, finished product drying and finished product packing are common process, wherein washing is to produce the shirt of sewing by washing off The impurity remained in journey is washed off;Drying is that the shirt after washing is dried to drying at 60 DEG C;It is pre- to scald for making clothes into blank, to carry High follow-up production efficiency, also repairs the fault produced in apparel manufacture;Pressing is to carry out pressing to each position of shirt, the time and Depending on temperature, pressure are according to fabric and shirt position, conventional pressing pressure is 3~5Kg, and 90~150 DEG C of pressing temperature, during pressing Between 15~35 seconds;Finished product is washed for removing the chemical substance remained in production process, further to improve its feel;Finished product drying Shirt after finished product is washed is dried to drying at 60 DEG C.
Advantage for present invention is:The formaldehydeless wash-and-wear of shirt of present invention production have good hydrophilic, moisture absorption and Breathability;The formaldehydeless generation in whole shirt production process simultaneously, finished product wash-and-wear of shirt are not remained containing formaldehyde yet, and finished product is exempted from The various strength losses of boiling hot shirt are than the few half of common ready-made non-ironing garment.
Specific embodiment
Example 1, the formaldehydeless wash-and-wear of shirt of textile 80/2 plain weave of production, its production stage are followed successively by shirt sewing, washing, dry Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 80%, the component of described formaldehyde-free durable-press finishing liquid It is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, no-ironing resin is dense in formaldehyde-free durable-press finishing liquid Spend for 180g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid is 40g/ L, and softening agent is formaldehydeless non-ironing whole Concentration in reason liquid is 50g/ L, and concentration of the catalyst in formaldehyde-free durable-press finishing liquid is 20g/ L;No-ironing resin is Germany The Arkofix NZK of CLARIANT companies, fiber protection agent is the Ceranine HDP. of German CLARIANT companies, softening agent For the Solusoft MW of German CLARIANT companies, catalyst is the Catalyst NKC of German CLARIANT companies;
Drying is that the shirt after washing is dried to drying at 60 DEG C;
The temperature of preliminary drying is 50 DEG C, and after preliminary drying, the liquid carrying rate of shirt is 40%;
The temperature for baking is 150 DEG C, and the time is 4 minutes;
The temperature of freezing is 5 DEG C, and the time is 1 hour, and the humidity of refrigerating chamber is 80%;
Shirt after finished product is washed by finished product drying is dried to drying at 60 DEG C.
The formaldehydeless wash-and-wear of shirt of finished product of the production of embodiment 1, content of formaldehyde are detected as 0.
Example 2, the formaldehydeless wash-and-wear of shirt of textile 100/2 twill of production, its production stage are followed successively by shirt sewing, washing, dry Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 80%, the component of described formaldehyde-free durable-press finishing liquid It is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, no-ironing resin is dense in formaldehyde-free durable-press finishing liquid Spend for 190g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid is 40g/ L, and softening agent is formaldehydeless non-ironing whole Concentration in reason liquid is 50g/ L, and concentration of the catalyst in formaldehyde-free durable-press finishing liquid is 30g/ L;No-ironing resin is Holland The protorez ffo of tanatex companies;Fiber protection agent is the persoftal pe25 of Dutch tanatex companies;
DICRYLAN WK of the softening agent for HUNTSMAN companies of the U.S.;KNITEX of the catalyst for HUNTSMAN companies of the U.S. MO;
Drying is that the shirt after washing is dried to drying at 60 DEG C;
The temperature of preliminary drying is 50 DEG C, and after preliminary drying, the liquid carrying rate of shirt is 40%;
The temperature for baking is 150 DEG C, and the time is 4 minutes;
The temperature of freezing is 5 DEG C, and the time is 1 hour, and the humidity of refrigerating chamber is 75%;
Shirt after finished product is washed by finished product drying is dried to drying at 60 DEG C.
The formaldehydeless wash-and-wear of shirt of finished product of the production of embodiment 2, content of formaldehyde are detected as 0.
Example 3, the formaldehydeless wash-and-wear of shirt of production 80/20 twill of polyester-cotton blend, its production stage are followed successively by shirt sewing, washing, dry Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 80%, the component of described formaldehyde-free durable-press finishing liquid It is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, no-ironing resin is dense in formaldehyde-free durable-press finishing liquid Spend for 180g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid is 40g/ L, and softening agent is formaldehydeless non-ironing whole Concentration in reason liquid is 50g/ L, and concentration of the catalyst in formaldehyde-free durable-press finishing liquid is 30g/ L;No-ironing resin is the U.S. The KNITEX FF of HUNTSMAN companies;Perapret additive peb of the fiber protection agent for BASF Corp. of Germany;
DICRYLAN WK of the softening agent for HUNTSMAN companies of the U.S.;KNITEX of the catalyst for HUNTSMAN companies of the U.S. MO;
Drying is that the shirt after washing is dried to drying at 60 DEG C;
The temperature of preliminary drying is 50 DEG C, and after preliminary drying, the liquid carrying rate of shirt is 40%;
The temperature for baking is 150 DEG C, and the time is 4 minutes;
The temperature of freezing is 5 DEG C, and the time is 1 hour, and the humidity of refrigerating chamber is 75%;
Shirt after finished product is washed by finished product drying is dried to drying at 60 DEG C.
The formaldehydeless wash-and-wear of shirt of finished product of the production of embodiment 3, content of formaldehyde are detected as 0.
Example 4, the formaldehydeless wash-and-wear of shirt of production 80/20 plain weave of polyester-cotton blend, its production stage are followed successively by shirt sewing, washing, dry Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 75%, the component of described formaldehyde-free durable-press finishing liquid It is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, no-ironing resin is dense in formaldehyde-free durable-press finishing liquid Spend for 200g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid is 45g/ L, and softening agent is formaldehydeless non-ironing whole Concentration in reason liquid is 55g/ L, and concentration of the catalyst in formaldehyde-free durable-press finishing liquid is 25g/ L;No-ironing resin is big for meaning The REACEL ZF of sharp BOZZETTO companies;Fiber protection agent is the WELLIN PE of Italian BOZZETTO companies;
Softening agent is the SEBOSAN SNC of Italian BOZZETTO companies;Catalyst is the CATAL of Italian BOZZETTO companies MCA;
Drying is that the shirt after washing is dried to drying at 60 DEG C;
The temperature of preliminary drying is 50 DEG C, and after preliminary drying, the liquid carrying rate of shirt is 40%;
The temperature for baking is 150 DEG C, and the time is 4 minutes;
The temperature of freezing is 5 DEG C, and the time is 1 hour, and the humidity of refrigerating chamber is 75%;
Shirt after finished product is washed by finished product drying is dried to drying at 60 DEG C.
The formaldehydeless wash-and-wear of shirt of finished product of the production of embodiment 4, content of formaldehyde are detected as 0.
Example 5, the formaldehydeless wash-and-wear of shirt of textile 120/2 plain weave of production, its production stage are followed successively by shirt sewing, washing, dry Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 70%, the component of described formaldehyde-free durable-press finishing liquid It is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, no-ironing resin is dense in formaldehyde-free durable-press finishing liquid Spend for 220g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid is 45g/ L, and softening agent is formaldehydeless non-ironing whole Concentration in reason liquid is 40g/ L, and concentration of the catalyst in formaldehyde-free durable-press finishing liquid is 35g/ L;No-ironing resin is Germany The Fixapret NF of BASF AG;Perapret additive peb of the fiber protection agent for BASF Corp. of Germany;Softening agent For the Sliligen sih of BASF Corp. of Germany;Fixapret f-m of the catalyst for BASF Corp. of Germany;
Drying is that the shirt after washing is dried to drying at 60 DEG C;
The temperature of preliminary drying is 50 DEG C, and after preliminary drying, the liquid carrying rate of shirt is 40%;
The temperature for baking is 150 DEG C, and the time is 4 minutes;
The temperature of freezing is 5 DEG C, and the time is 1 hour, and the humidity of refrigerating chamber is 80%;
Shirt after finished product is washed by finished product drying is dried to drying at 60 DEG C.
The formaldehydeless wash-and-wear of shirt of finished product of the production of embodiment 5, content of formaldehyde are detected as 0.

Claims (2)

1. a kind of production method of formaldehydeless wash-and-wear of shirt, it is characterised in that production stage is followed successively by shirt sewing, washing, dries Dry, sprinkling formaldehyde-free durable-press finishing liquid, preliminary drying, it is pre- scald, pressing, bake, freeze, finished product washing, finished product drying and finished product packing;
Wherein spray formaldehyde-free durable-press finishing liquid be to carry out formaldehyde-free durable-press finishing liquid atomized spray to shirt, it is ensured that clothes each Position is all sprayed with formaldehyde-free durable-press finishing, makes the liquid carrying rate of shirt reach 65~90%, described formaldehyde-free durable-press finishing liquid Component is made up of no-ironing resin, fiber protection agent, softening agent, catalyst and water, and no-ironing resin is in formaldehyde-free durable-press finishing liquid Concentration be 150~240g/ L, concentration of the fiber protection agent in formaldehyde-free durable-press finishing liquid be 30~50g/ L, softening agent Concentration in formaldehyde-free durable-press finishing liquid be 20~60g/ L, concentration of the catalyst in formaldehyde-free durable-press finishing liquid be 15~ 35g/ L;
The temperature of preliminary drying is 40~60 DEG C, and after preliminary drying, the liquid carrying rate of shirt reaches 20~50%;
The temperature for baking is 140~160 DEG C, and the time is 3~7 minutes;
Freezing is that the shirt after baking is put into refrigerating chamber freezing, and the temperature of freezing is 10~0 DEG C, cooling time is 0.5~ 1.5 hours, the humidity of refrigerating chamber was 60~90%.
2. the production method of formaldehydeless wash-and-wear of shirt according to claim 1, it is characterised in that in formaldehyde-free durable-press finishing In liquid, no-ironing resin is Arkofix NZK, protorez ffo, KNITEX FF, REACEL ZF or Fixapret NF;Fiber Protective agent is Ceranine HDP., persoftal pe25, WELLIN PE or Perapret additive peb;Softening agent For Solusoft MW, SE1, persoftal sme, DICRYLAN WK, SEBOSAN SNC or Sliligen sih;Catalyst For Catalyst NKC, KNITEX MO, CATAL MCA or Fixapret f-m.
CN201611189960.2A 2016-12-21 2016-12-21 Production method of formaldehyde-free wash-and-wear shirt Pending CN106510007A (en)