CN105239422A - 酒红色活性染料组合物及染色工艺 - Google Patents

酒红色活性染料组合物及染色工艺 Download PDF

Info

Publication number
CN105239422A
CN105239422A CN201510754339.5A CN201510754339A CN105239422A CN 105239422 A CN105239422 A CN 105239422A CN 201510754339 A CN201510754339 A CN 201510754339A CN 105239422 A CN105239422 A CN 105239422A
Authority
CN
China
Prior art keywords
minutes
dye
clear water
fixation
add
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510754339.5A
Other languages
English (en)
Inventor
周文江
董建刚
顾景春
吴星星
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WUXI HODOHOME GARMENT CO Ltd
Original Assignee
WUXI HODOHOME GARMENT CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUXI HODOHOME GARMENT CO Ltd filed Critical WUXI HODOHOME GARMENT CO Ltd
Priority to CN201510754339.5A priority Critical patent/CN105239422A/zh
Publication of CN105239422A publication Critical patent/CN105239422A/zh
Pending legal-status Critical Current

Abstract

本发明涉及一种酒红色活性染料组合物及染色工艺,其特征是,包括以下步骤:(1)向染缸中进布,加入烧碱、去油灵和精炼剂,加热至70~75℃时加入双氧水,加热至98~100℃漂棉10~15分钟;(2)经步骤(1)漂棉后用清水洗涤,加热至60~65℃向染缸中加入元明粉,接着升温至65~70℃缓慢加入搅拌均匀的染料;接着加入纯碱,保温10~12分钟;所述染色浴比为1:7~8,(3)固色:经步骤(2)后向染缸中加入20±1%o.w.f纯碱,纯碱在10~15分钟内加完,固色40~45分钟,固色pH值为10~11;(4)固色后经清水洗涤、过酸、清水洗涤、皂洗、清水洗涤、过酸后出缸。本发明减少深色织物染料的用量,避免色花的产生,增加了染料的利用率,降低了污水的排入。

Description

酒红色活性染料组合物及染色工艺
技术领域
本发明涉及一种酒红色活性染料组合物及染色工艺,属于活性染料染色方法技术领域。
背景技术
活性染料是染料行业里最重要和主要的一大类,活性染料上染过程中首先吸附在纤维表面,然后向纤维内部扩散,由于固着阶段染料与纤维的键破坏了已达到的吸附平衡,且碱剂亦为促染剂,染料进一步被吸附,促使染料更多地与纤维结合。
由于活性染料亲和力普遍较低,一般要用大量元明粉或食盐促染,为防止染料水解,上染一般在中性条件下进行。
活性染料的固着是指活性染料与棉纤维的反应在碱性条件下,纤维素能形成纤维素负离子,能和活性染料发生亲核取代、加成反应,进而形成染料—纤维共价键,二氯均三嗪型较活泼,只需在较低温度下即可反应,而一氯均三嗪型则需在温度较高、碱性较强条件下才能反应。影响此反应的因素有很多。染料与纤维与水的反应为平行反应,因为水也是亲核试剂,反应条件机理相同。染料一经水解即失去与纤维的反应能力,固色率大为降低。从反应动力学研究得到,固着反应比水解反应快40倍左右,染色时pH一般为10~11为宜,X型可用碱性较弱的小苏打;对K型,则采用Na2CO3、Na3PO4,甚至NaOH。染色温度具体根据不同染料性能而定。促染用元明粉,加入要掌握一多二早,分批加入的原则。浴比尽可能小些,以提高固色率。水解染料的存在,对纤维有一定的亲和力,但不够大,它会染着于纤维上,皂煮时不能完全煮下来,有时还会污染到其它纤维,特别是KN型染料耐碱牢度不高,易造成污染现象。水解染料的存在也是湿摩牢度较低的重要原因。
现有技术中,深色织物染料用量一般比较大,并且存在色花的现象;另外,活性染料染色过程会产生大量的染色污水排放。
发明内容
本发明的目的是克服现有技术中存在的不足,提供一种酒红色活性染料组合物及染色工艺,减少深色织物染料的用量,避免色花的产生,增加了染料的利用率,降低了污水的排入。
按照本发明提供的技术方案,所述酒红色活性染料组合物,其特征是,包括以下组份:活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB、活性橙LC-4RN和元青B133的质量比为1.95:1.05:0.44。
所述染色工艺,其特征是,包括以下步骤:
(1)向染缸中进布,加入3~3.5g/L烧碱、1.5~2g/L去油灵和2~2.5g/L精炼剂,加热至70~75℃时加入6~7g/L双氧水,加热至98~100℃漂棉10~15分钟;
(2)染色:经步骤(1)漂棉后用清水洗涤2~3遍,加热至60~65℃向染缸中加入50±1%o.w.f元明粉,接着升温至65~70℃缓慢加入搅拌均匀的染料,染料在10~15分钟内加完;接着加入1.2~1.3%o.w.f纯碱,纯碱在10~15分钟内加完,保温10~12分钟;所述染色浴比为1:7~8,所述染料包括活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB的用量为1.95%o.w.f±0.5mg,活性橙LC-4RN的用量为1.05%o.w.f±0.5mg,元青B133的用量为0.44%o.w.f±0.5mg;
(3)固色:经步骤(2)后向染缸中加入20±1%o.w.f纯碱,纯碱在10~15分钟内加完,固色40~45分钟,固色pH值为10~11;
(4)固色后经清水洗涤、过酸、清水洗涤、皂洗、清水洗涤、过酸后出缸。
进一步的,所述布为针织氨纶棉毛布。
进一步的,所述清水洗涤每次洗1~2遍。
进一步的,所述皂洗时加入皂洗液,皂洗温度为85~95℃,洗涤时间为10~15分钟。
本发明所述的酒红色活性染料组合物及染色工艺,可以解决染色困难的问题,也使整理后面料的牢度提高。
具体实施方式
下面结合具体实施例对本发明作进一步说明。
本发明所使用的活性红LC-DB、活性橙LC-4RN均购自江苏江阴帝安化工有限公司。
实施例一:一种染色工艺,包括以下步骤:
(1)向染缸中进布,加入3g/L烧碱、1.5g/L去油灵和2g/L精炼剂,加热至70℃时加入6g/L双氧水,加热至98℃漂棉15分钟;所述布为针织氨纶棉毛布;
(2)染色:经步骤(1)漂棉后用清水洗涤2遍,加热至60℃向染缸中加入49%o.w.f元明粉,接着升温至65℃缓慢加入搅拌均匀的染料,染料在15分钟内加完;接着加入1.2%o.w.f纯碱,纯碱在15分钟内加完,保温12分钟;所述染色浴比为1:7,所述染料包括活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB的用量为1.95%o.w.f,活性橙LC-4RN的用量为1.05%o.w.f,元青B133的用量为0.44%o.w.f;
(3)固色:经步骤(2)后向染缸中加入19%o.w.f纯碱,纯碱在15分钟内加完,固色45分钟,固色pH值为10;
(4)固色后经清水洗涤1遍、过酸、清水洗涤洗1遍;
(5)皂洗:皂洗温度为85℃,洗涤时间为15分钟;
(6)清水洗涤1遍、过酸后出缸。
所述面料色牢度检测如下:干摩擦牢度为4级,湿摩擦牢度为4级,皂洗牢度为3-4级,沾色牢度为4级。
实施例二:一种染色工艺,包括以下步骤:
(1)向染缸中进布,加入3.5g/L烧碱、2g/L去油灵和2.5g/L精炼剂,加热至75℃时加入7g/L双氧水,加热至100℃漂棉10分钟;所述布为针织氨纶棉毛布;
(2)染色:经步骤(1)漂棉后用清水洗涤3遍,加热至65℃向染缸中加入51%o.w.f元明粉,接着升温至70℃缓慢加入搅拌均匀的染料,染料在10分钟内加完;接着加入1.3%o.w.f纯碱,纯碱在10分钟内加完,保温10分钟;所述染色浴比为1:8,所述染料包括活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB的用量为1.95%o.w.f,活性橙LC-4RN的用量为1.05%o.w.f,元青B133的用量为0.44%o.w.f;
(3)固色:经步骤(2)后向染缸中加入21%o.w.f纯碱,纯碱在10分钟内加完,固色40分钟,固色pH值为11;
(4)固色后经清水洗涤2遍、过酸、清水洗涤洗2遍;
(5)皂洗:皂洗温度为95℃,洗涤时间为10分钟;
(6)清水洗涤2遍、过酸后出缸。
所述面料色牢度检测如下:干摩擦牢度为4级,湿摩擦牢度为4级,皂洗牢度为3-4级,沾色牢度为4级。
实施例三:一种染色工艺,包括以下步骤:
(1)向染缸中进布,加入3.2g/L烧碱、1.6g/L去油灵和2.4g/L精炼剂,加热至72℃时加入6.5g/L双氧水,加热至99℃漂棉12分钟;所述布为针织氨纶棉毛布;
(2)染色:经步骤(1)漂棉后用清水洗涤2遍,加热至62℃向染缸中加入50%o.w.f元明粉,接着升温至66℃缓慢加入搅拌均匀的染料,染料在12分钟内加完;接着加入1.2%o.w.f纯碱,纯碱在12分钟内加完,保温11分钟;所述染色浴比为1:7,所述染料包括活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB的用量为1.95%o.w.f,活性橙LC-4RN的用量为1.05%o.w.f,元青B133的用量为0.44%o.w.f;
(3)固色:经步骤(2)后向染缸中加入20%o.w.f纯碱,纯碱在12分钟内加完,固色42分钟,固色pH值为10;
(4)固色后经清水洗涤2遍、过酸、清水洗涤洗2遍;
(5)皂洗:皂洗温度为90℃,洗涤时间为12分钟;
(6)清水洗涤2遍、过酸后出缸。
所述面料色牢度检测如下:干摩擦牢度为4级,湿摩擦牢度为4级,皂洗牢度为3-4级,沾色牢度为4级。

Claims (5)

1.一种酒红色活性染料组合物,其特征是,包括以下组份:活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB、活性橙LC-4RN和元青B133的质量比为1.95:1.05:0.44。
2.一种染色工艺,其特征是,包括以下步骤:
(1)向染缸中进布,加入3~3.5g/L烧碱、1.5~2g/L去油灵和2~2.5g/L精炼剂,加热至70~75℃时加入6~7g/L双氧水,加热至98~100℃漂棉10~15分钟;
(2)染色:经步骤(1)漂棉后用清水洗涤2~3遍,加热至60~65℃向染缸中加入50±1%o.w.f元明粉,接着升温至65~70℃缓慢加入搅拌均匀的染料,染料在10~15分钟内加完;接着加入1.2~1.3%o.w.f纯碱,纯碱在10~15分钟内加完,保温10~12分钟;所述染色浴比为1:7~8,所述染料包括活性红LC-DB、活性橙LC-4RN和元青B133,活性红LC-DB的用量为1.95%o.w.f±0.5mg,活性橙LC-4RN的用量为1.05%o.w.f±0.5mg,元青B133的用量为0.44%o.w.f±0.5mg;
(3)固色:经步骤(2)后向染缸中加入20±1%o.w.f纯碱,纯碱在10~15分钟内加完,固色40~45分钟,固色pH值为10~11;
(4)固色后经清水洗涤、过酸、清水洗涤、皂洗、清水洗涤、过酸后出缸。
3.如权利要求2所述的染色工艺,其特征是:所述布为针织氨纶棉毛布。
4.如权利要求2所述的染色工艺,其特征是:所述清水洗涤每次洗1~2遍。
5.如权利要求2所述的染色工艺,其特征是:所述皂洗时加入皂洗液,皂洗温度为85~95℃,洗涤时间为10~15分钟。
CN201510754339.5A 2015-11-09 2015-11-09 酒红色活性染料组合物及染色工艺 Pending CN105239422A (zh)