CN103721857A - 一种硅锌矿物捕收剂的制备方法 - Google Patents

一种硅锌矿物捕收剂的制备方法 Download PDF

Info

Publication number
CN103721857A
CN103721857A CN201310751000.0A CN201310751000A CN103721857A CN 103721857 A CN103721857 A CN 103721857A CN 201310751000 A CN201310751000 A CN 201310751000A CN 103721857 A CN103721857 A CN 103721857A
Authority
CN
China
Prior art keywords
willemite
collecting agent
mineral
mixture
heating
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201310751000.0A
Other languages
English (en)
Other versions
CN103721857B (zh
Inventor
穆枭
陈建华
陈晔
李玉琼
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangxi University
Original Assignee
Guangxi University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangxi University filed Critical Guangxi University
Priority to CN201310751000.0A priority Critical patent/CN103721857B/zh
Publication of CN103721857A publication Critical patent/CN103721857A/zh
Application granted granted Critical
Publication of CN103721857B publication Critical patent/CN103721857B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种硅锌矿物捕收剂的制备方法,包括如下步骤:以大豆、蓖麻耔、茶树耔和茶树树皮中的两种或三种为原料。经烘干、粉碎和过筛,按质量比取:果树皮粉末:三乙醇胺:水=5~8:2~4:5~10,加热至120~130℃,通入氮气搅拌反应2~3h,再升温至150~160℃,通入氮气搅拌反应2~3h,冷却至60℃以下,取滤液用离心沉淀机进行2~3次离心分离。上层清液进行减压蒸馏,得深黄色浓缩液,在60~70℃水浴中加热,将溶剂蒸干,完全干燥后得到黄色粉末即为硅锌矿矿物的捕收剂。采用本发明所述捕收剂能够有效捕收泥化、含白云石的硅锌矿物。

Description

一种硅锌矿物捕收剂的制备方法
一、技术领域
本发明涉及一种硅锌矿矿物的捕收剂,特别是对于含泥和含白云石脉石的硅锌矿。
二、背景技术
氧化锌矿种类繁多,常见的有工业价值的氧化锌矿物是菱锌矿(ZnC03)和异极矿[ZnSi2O7·(OH)2·H2O]、硅锌矿(ZnSiO3)、水锌矿[3Zn(OH)2·2ZnCO3]、红锌矿(ZnO)等。菱锌矿和异极矿的回收,目前最有效的方法是硫化胺浮选法。硅锌矿往往与菱锌矿共存,长期以来,由于硅锌矿物难捕收,在回收氧化锌矿时常常不能有效回收,造成了极大的资源浪费。
三、发明内容
本发明的目的在于提供一种硅锌矿物捕收剂的制备方法,制备得的捕收剂能够有效捕收泥化、含白云石的硅锌矿物,药剂用量少,无毒无污染。
本发明采用以下技术方案达到上述目的:一种硅锌矿物捕收剂的制备方法,包括如下步骤:以植物果实、果皮或树皮为原料,洗净后低温烘干、粉碎,过100目筛,按质量比取:果树皮粉末:三乙醇胺:水=5~8:2~4:5~10,加热至120~130℃,通入氮气搅拌反应2~3h,再升温至150~160℃,通入氮气搅拌反应2~3h,冷却至60℃以下,过滤3~5次,取滤液用离心沉淀机进行2~3次离心分离,上层清液进行减压蒸馏,得深黄色浓缩液,在60~70℃水浴中加热,将溶剂蒸干,得到的粘稠液体在温度为60℃的真空干燥箱中干燥,得到黄褐色粘稠固体,完全干燥后得到黄色粉末即为硅锌矿矿物的捕收剂。
所述果树皮原料为蓖麻耔、茶油耔、大豆和茶树树皮中的两种或三种。
浮选时,矿浆pH值为12~13,浮选过程中,将矿石磨矿至矿物单体解离后,加入分散剂、抑制剂和活化剂,按1000~1500g/t加入所述捕收剂,然后再加起泡剂。
使用时,将所述抑制剂先配制成质量百分浓度为1~3%的水溶液。
药剂总用量为:1000~1500g/t。
本发明的具体优点在于:
1、采用本发明制备的捕收剂能够对含泥、白云石脉石矿物硅锌矿进行较好的捕收作用,使有用矿物获得较好的回收率和精矿品位。
2、药剂用量少,无毒无污染。
四、具体实施方式
以下通过具体实施例对本发明的技术方案作进一步描述。
实施例1
本发明所述硅锌矿物捕收剂的制备方法的一个实例,包括以下步骤:
以茶树耔、蓖麻耔和茶树树皮为原料,洗净后低温烘干、粉碎,过100目筛,得所述果皮粉末,按质量比取:果皮粉末:三乙醇胺:水=6:4:10,加热至120℃,通入氮气搅拌反应2h,再升温至150~160℃,通入氮气搅拌反应2~3h,用冷水浴冷却至60℃以下,用纱布过滤5次,取滤液用离心沉淀机进行2~3次离心分离,上层清液收集于圆底烧瓶中进行减压蒸馏,得深黄色浓缩液,在温度为60~70℃水浴中加热,将溶剂蒸干,得到的粘稠液体在真空干燥箱中干燥,温度60℃左右,将溶剂蒸干,得到的粘稠液体在温度60℃的真空干燥箱中干燥,得到黄褐色粘稠固体,完全干燥后得到有特殊香味的黄色粉末即为硅锌矿物的捕收剂。
实施例2
本发明所述硅锌矿物捕收剂的制备方法的一个实例,包括以下步骤:
以大豆、蓖麻耔和茶树树皮为原料,洗净后低温烘干、粉碎,过100目筛,得所述果皮粉末,按质量比取:果皮粉末:三乙醇胺:水=6:4:10,加热至120℃,通入氮气搅拌反应保持2h,再升温至150~160℃,通入氮气搅拌反应2~3h,用冷水浴冷却至60℃以下,用纱布过滤5次,取滤液用离心沉淀机进行2~3次离心分离,上层清液收集于圆底烧瓶中进行减压蒸馏,得深黄色浓缩液,在温度为60~70℃水浴中加热,将溶剂蒸干,得到的粘稠液体在温度为60℃的真空干燥箱中干燥,将溶剂蒸干,得到黄褐色粘稠固体,完全干燥后得到有特殊香味的黄色粉末即为硅锌矿物的捕收剂。
实施例3
本实施例为所述硅锌矿物捕收剂在硅锌矿矿物浮选中的应用实例。
1、矿物原料:
原料矿石中硅锌矿中锌含量为10.2%,铁3.17%,铁主要以褐铁矿形式存在,矿石泥化严重。物相分析表明锌主要是以硅锌矿形式存在。
2、药剂制度及操作条件:用碳酸钠调矿浆pH到12~13、按六偏磷酸钠2000g/t,硫酸铜200g/t,捕收剂用量1200g/t,2号油60g/t药剂用量进行了一年100t/d工业扩大试验,结果表明采用以上工艺和药剂条件能够有效将泥化硅锌矿浮选回收,在给矿锌品位为10.2%条件下,经过一次粗选两次扫选及二次精选,浮选精矿锌品位可以达到45.8%,回收率达到80.25%。
实施例4
本实施例为所述硅锌矿物捕收剂在硅锌矿矿物浮选中的应用实例。
1、矿物原料
原料矿石中硅锌矿中锌含量为8.2%,白云石8.24%,铁主要以褐铁矿形式存在,矿石泥化严重。物相分析表明锌主要是以硅锌矿形式存在。
2、药剂制度及操作条件:碳酸钠调矿浆pH到12~13.5,按照捕收剂1300g/t,六偏磷酸钠3000g/t,硫酸铜200g/t,2号油80g/t的药剂用量进行了八个月200t/d的工业试验,结果表明采用上述工艺和药剂条件能够有效回收硅锌矿物,经过一次粗选两次扫选及二次精选,得到铅锑品位达到43.65%,回收率达到81.26%的浮选精矿。

Claims (4)

1.一种硅锌矿物捕收剂的制备方法,其特征在于,包括如下步骤:以植物果实、果皮或树皮为原料,洗净后低温烘干、粉碎,过100目筛,按质量比取:果树皮粉末:三乙醇胺:水=5~8:2~4:5~10,加热至120~130℃,通入氮气搅拌反应2~3h,再升温至150~160℃,通入氮气搅拌反应2~3h,冷却至60℃以下,过滤3~5次,取滤液用离心沉淀机进行2~3次离心分离,上层清液进行减压蒸馏,得深黄色浓缩液,在60~70℃水浴中加热,将溶剂蒸干,得到的粘稠液体在温度为60℃的真空干燥箱中干燥,得到黄褐色粘稠固体,完全干燥后得到黄色粉末即为硅锌矿矿物的捕收剂。
2.根据权利要求1所述的硅锌矿物捕收剂的制备方法,其特征在于,所述果树皮原料为蓖麻耔、茶油耔、大豆和茶树树皮中的两种或三种。
3.权利要求1所述硅锌矿物捕收剂的应用,其特征在于,浮选时用碳酸钠调矿浆pH值为12~13,浮选过程中,将矿石磨矿至矿物单体解离后,加入分散剂、抑制剂和活化剂,按捕收剂用量为1000~1500g/t加入所述捕收剂,然后再加起泡剂。
4.根据权利要求2所述硅锌矿物捕收剂的应用,其特征在于,使用时,将所述抑制剂先配制成质量百分浓度为1~3%的水溶液。
CN201310751000.0A 2013-12-31 2013-12-31 一种硅锌矿物捕收剂的制备方法 Expired - Fee Related CN103721857B (zh)