CN103386420A - 一种冷轧带钢穿带方法 - Google Patents

一种冷轧带钢穿带方法 Download PDF

Info

Publication number
CN103386420A
CN103386420A CN2013103177935A CN201310317793A CN103386420A CN 103386420 A CN103386420 A CN 103386420A CN 2013103177935 A CN2013103177935 A CN 2013103177935A CN 201310317793 A CN201310317793 A CN 201310317793A CN 103386420 A CN103386420 A CN 103386420A
Authority
CN
China
Prior art keywords
strip steel
coiled strip
milling train
rolling
rolling mill
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2013103177935A
Other languages
English (en)
Other versions
CN103386420B (zh
Inventor
杨东
王树胜
李春明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanxi Taigang Stainless Steel Co Ltd
Original Assignee
Shanxi Taigang Stainless Steel Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanxi Taigang Stainless Steel Co Ltd filed Critical Shanxi Taigang Stainless Steel Co Ltd
Priority to CN201310317793.5A priority Critical patent/CN103386420B/zh
Publication of CN103386420A publication Critical patent/CN103386420A/zh
Application granted granted Critical
Publication of CN103386420B publication Critical patent/CN103386420B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开一种冷轧带钢穿带方法,属于带钢轧制领域。该方法包括:(1)在上一卷带钢轧制结束、带尾脱离钳口后,不急于将带尾拉过轧机;(2)开卷工进行下一卷带钢的送料操作,将下一卷带钢头部送至轧机入口刮油辊外侧;(3)当上一卷带钢尾部与后一卷带钢头部上下搭接后,使其开卷机运行速度V开卷与轧机运行速度V轧机相等;(4)待下一卷带钢头部随上一卷带钢的尾部顺利穿过轧机到达轧机出口导向辊处,开卷工停止送料;(5)卷取上一卷带钢的尾部,将上一卷带钢尾部卷取到钢卷上。该方法在二十辊轧机穿带过程中,避免了冷轧带钢带头插入轧机工作辊与中间辊辊缝间隙或轧机喷油导板下,实现了顺利穿带操作。

Description

一种冷轧带钢穿带方法
技术领域
本发明涉及一种冷轧带钢穿带方法,属于带钢轧制领域。
背景技术
冷轧带钢在轧机上第一道开卷过程中,头部由于重力和卷取原因,总是向下钩。因而在穿带过程中,头部易插入轧机工作辊与中间辊辊缝间隙或轧机喷油导板下,造成不能顺利穿带,并且损坏工作辊表面。需机前工使用专用工具,协同穿带操作。这样,不但影响穿带时间,而且损坏的工作辊表面,严重影响产品表面质量。
发明内容
为了克服上述不足,本发明旨在提供一种冷轧带钢穿带方法,使冷轧带钢在二十辊轧机穿带过程中,带头不易插入轧机工作辊与中间辊辊缝间隙或轧机喷油导板下,实现顺利穿带。
本发明提供的一种冷轧带钢穿带方法,包括以下步骤:
(1)在上一卷带钢轧制结束、带尾脱离钳口后,不急于将带尾拉过轧机,使其尾部位于轧机入口转向辊外0.5米;
(2)这时,开卷工进行下一卷带钢的送料操作,将下一卷带钢头部送至轧机入口刮油辊外侧。此时,前后两卷带钢形成了上下搭接;
(3)当上一卷带钢尾部与后一卷带钢头部上下搭接后,由主操作工更改人机界面中开卷机和轧机运行速度,使其V开卷=V轧机=20米/分(V开卷即开卷机运行速度,V轧机即轧机运行速度);这时,开卷机和轧机同时运行,实现前后两卷带钢同步向前运动。这样,借助上一卷带钢尾部的拖动、引导及下一卷带钢的同步送料操作,实现快速穿带操作。
(4)待下一卷带钢头部随上一卷带钢的尾部顺利穿过轧机到达轧机出口导向辊处,开卷工停止送料;
(5)卷取上一卷带钢的尾部,将上一卷带钢尾部卷取到钢卷上,卸卷后,进行下一卷带钢的送料和咬钳口操作,成功实现下一卷带钢的穿带操作。
本发明的操作关键在于:(1)在上一卷带钢轧制结束时,不将带尾拉过轧机,提前对下一卷带钢进行穿带送料操作,上一卷带钢尾部与后一卷带钢头部搭接后,前后带钢要同步运行,避免前后带钢速度不同,表面搓擦,形成表面划伤或搭接脱落,不能顺利穿带;(2)当上一卷带钢尾部与后一卷带钢头部搭接后,由主操作工更改人机界面中开卷机和轧机运行速度,使其V开卷=V轧机=20米/分(V开卷即开卷机运行速度,V轧机即轧机运行速度);这时,开卷机和轧机同时运行,实现前后两卷带钢同步向前运动。这样,借助上一卷带钢尾部的拖动、引导及下一卷带钢的同步送料操作,实现快速穿带操作,轧机穿带速度和卷取速度会变成一样,就能实现前后带钢同步运行。
本发明的有益效果:
使用“前后搭接”穿带方法,使冷轧带钢在二十辊轧机穿带过程中,带头不易插入轧机工作辊与中间辊辊缝间或轧机喷油导板下,不仅实现了快速顺利穿带,而且有效解决了穿带损坏工作辊表面问题,减少了带钢表面质量缺陷。
附图说明
图1为现有技术中穿带操作示意图。
图2为现有技术中穿带操作示意图。
图3为本发明提供的穿带方法示意图。
图中1为支撑辊,2为中间辊,3为工作辊,4为带钢头部,5为喷油导板,6为上一卷带钢尾部,7为下一卷带钢头部。
具体实施方式
下面通过实施例来进一步说明本发明,但不局限于以下实施例。
实施例:
图1、图2示出了现有技术中穿带操作示意图。图1中,带钢头部4插入到了工作辊3与中间辊2辊缝间隙,图2中,带钢头部4插入到了喷油导板5下面,均造成不能顺利穿带,并且损坏工作辊表面。
图3为本发明提供的穿带方法示意图。上一卷带钢尾部6与下一卷带钢头部7形成上下搭接之式。该方法包括以下步骤:
(1)在上一卷带钢轧制结束、带尾脱离钳口后,不急于将带尾拉过轧机,使其尾部位于轧机入口转向辊外0.5米;
(2)这时,开卷工进行下一卷带钢的送料操作,将下一卷带钢头部送至轧机入口刮油辊外侧,此时,前后两卷带钢形成了上下搭接;
(3)当上一卷带钢尾部与后一卷带钢头部上下搭接后,由主操作工更改人机界面中开卷机和轧机运行速度,使其V开卷=V轧机=20米/分(V开卷即开卷机运行速度,V轧机即轧机运行速度);这时,开卷机和轧机同时运行,实现前后两卷带钢同步向前运动,这样,借助上一卷带钢尾部的拖动、引导及下一卷带钢的同步送料操作,实现快速穿带操作;
(4)待下一卷带钢头部随上一卷带钢的尾部顺利穿过轧机到达轧机出口导向辊处,开卷工停止送料;
(5)卷取上一卷带钢的尾部,将上一卷带钢尾部卷取到钢卷上,卸卷后,进行下一卷带钢的送料和咬钳口操作,成功实现下一卷带钢的穿带操作。
该方法现已在太钢不锈冷轧厂1-11#轧机上试用“前后搭接”穿带方法,不仅实现了快速顺利穿带,而且有效解决了穿带损坏工作辊表面问题,效果良好。

Claims (2)

1.一种冷轧带钢穿带方法,其特征在于:包括以下步骤:
(1)在上一卷带钢轧制结束、带尾脱离钳口后,不急于将带尾拉过轧机,使其尾部位于轧机入口转向辊外0.5米;
(2)开卷工进行下一卷带钢的送料操作,将下一卷带钢头部送至轧机入口刮油辊外侧,此时,前后两卷带钢形成了上下搭接;
(3)当上一卷带钢尾部与后一卷带钢头部上下搭接后,由主操作工更改人机界面中开卷机和轧机运行速度,使其开卷机运行速度V开卷与轧机运行速度V轧机相等;这时,开卷机和轧机同时运行,实现前后两卷带钢同步向前运动,借助上一卷带钢尾部的拖动、引导下一卷带钢的同步送料操作,实现快速穿带操作;
(4)待下一卷带钢头部随上一卷带钢的尾部顺利穿过轧机到达轧机出口导向辊处,开卷工停止送料;
(5)卷取上一卷带钢的尾部,将上一卷带钢尾部卷取到钢卷上,卸卷后,进行下一卷带钢的送料和咬钳口操作,成功实现下一卷带钢的穿带操作。
2.根据权利要求1所述的冷轧带钢穿带方法,其特征在于:所述步骤(3)中,开卷机运行速度V开卷与轧机运行速度V轧机为20米/分钟。
CN201310317793.5A 2013-07-26 2013-07-26 一种冷轧带钢穿带方法 Active CN103386420B (zh)