CN102999240B - Ogs玻璃的外形加工方法 - Google Patents

Ogs玻璃的外形加工方法 Download PDF

Info

Publication number
CN102999240B
CN102999240B CN201210542906.7A CN201210542906A CN102999240B CN 102999240 B CN102999240 B CN 102999240B CN 201210542906 A CN201210542906 A CN 201210542906A CN 102999240 B CN102999240 B CN 102999240B
Authority
CN
China
Prior art keywords
glass
ogs
layer
forming
ogs glass
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210542906.7A
Other languages
English (en)
Other versions
CN102999240A (zh
Inventor
朱君毅
陶力争
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fuzhou Lianchuang Electronic Co., Ltd
Original Assignee
Jiangxi Lianchuang Electronic Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangxi Lianchuang Electronic Co Ltd filed Critical Jiangxi Lianchuang Electronic Co Ltd
Priority to CN201210542906.7A priority Critical patent/CN102999240B/zh
Publication of CN102999240A publication Critical patent/CN102999240A/zh
Application granted granted Critical
Publication of CN102999240B publication Critical patent/CN102999240B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了OGS玻璃外形加工方法,在大张玻璃两面印刷和OGS玻璃外形相近的耐酸保护膜,通过氰氟酸等量蚀刻掉未保护区域,形成基板,将基板进行钢化处理,在其表面形成均匀的钢化层。钢化过的基板叫做母板。母板通过数道镀膜、黄光制程在其一面未曾蚀刻的区域形成油墨层和ITO线路层。具有油墨层和ITO层的母板称为功能片。接下来通过裁切取掉母版中凹槽的废料形成单片OGS玻璃半成品,最后通过CNC对裁切面进行打磨形成OGS玻璃成品。本发明的核心是确保了OGS玻璃表面钢化层的完整性,从而确保了OGS玻璃表面应力层的功能,从而确保了OGS电容触摸屏整体强度以及批量强度的均一性。

Description

OGS玻璃的外形加工方法
技术领域
 本发明涉及一种OGS(One glass solution)结构电容触摸屏,特别涉及OGS玻璃的裁切方法。
背景技术
目前市场上主流的电容屏由盖板玻璃、ITO(氧化铟锡)透明传感器、柔性电路板、控制芯片IC(控制集成芯片)、OCA(光学透明胶)、保护膜、电子元件构成,总体厚度超过0.9mm,透光率小于86%。OGS结构电容屏实现了盖板玻璃与触摸屏一体化,即OGS玻璃。省去了ITO 透明传感器、OCA,还省去了多次贴合过程,使得触摸屏成本下降约30%,整体厚度控制在0.7mm以内,透光率大于90%。同目前主流电容屏相比较,OGS电容屏更薄、透光率更高、成本更低,将成为未来触摸屏技术、市场发展的主流方向之一。
OGS结构电容触摸屏核心是OGS玻璃,即在保护玻璃上直接形成ITO导电膜及传感器的技术。一块玻璃同时起到保护玻璃和触摸传感器的双重作用,其厚度小于0.7mm,表面硬度≥7H,四点静压测试强度≥500MPa 。钢化玻璃的强度取决于玻璃表面的应力大小,应力的大小由钢化玻璃的钢化深度来决定,触摸屏玻璃的强化深度通常为0.008-0.015mm之间。目前行业内可批量生产的OGS玻璃的工艺按照镀膜、裁切的先后顺序,分为大片制程和小片制程两种。小片制程是指将大张玻璃通过裁切及CNC加工成OGS玻璃的外形后钢化,再经过数道镀膜、黄光制程,在玻璃的一面形成所要的颜色、图案和ITO线路,从而形成OGS玻璃成品;大片制程是先将大张玻璃强化,通过数道镀膜、黄光制程在玻璃的一面形成多片具有颜色、图案和ITO线路的OGS玻璃外形,再通过裁切、CNC加工、化学强化修复成多片OGS玻璃成品。OGS玻璃成品通过绑定FPC形成OGS电容触摸屏。小片制程由于是单片镀膜、黄光制程,效率很低,成本没有任何优势,不被大家所接受。大片制程,成本相对小片制程而言具有明显优势,也是目前各厂家首选的OGS触摸屏加工方案。但是大片制程由于涉及玻璃钢化后裁切和CNC加工,破坏了OGS玻璃钢化层的结构,在裁切断面离玻璃表面0.15mm深度的范围内形成无数细小的裂纹,这些细小的裂纹降低了OGS玻璃表面的应力值,从而降低了OGS结构触摸屏整体的强度。虽然通过增加化学强化的工序进行修复,但是产品强度均一性差,影响整体品质。
发明内容
本发明所要解决的技术问题是:提供一种OGS玻璃外形大片制程加工方法,在裁切断面离玻璃表面不会形成无数细小的裂纹,保证OGS玻璃表面钢化层的完整性,确保OGS玻璃表面应力层的功能以及OGS电容触摸屏整体强度和批量强度的均一性。
针对上述目的,本发明采取以下技术方案,OGS玻璃外形加工方法,其特征在于,其步骤如下:
1) 在大片玻璃正反两面印刷一一对应的OGS玻璃外形耐酸保护膜,耐酸保护膜尺寸比OGS玻璃外形尺寸单边大0.13mm~0.16mm;
2) 将大片玻璃浸泡在氰氟酸溶液中,进行等量蚀刻,氰氟酸浓度5%~30%(体积百分比),时间120min~150min,温度38℃~42℃,蚀刻深度为0.13mm~0.16mm,大张玻璃蚀刻后形成的基板正反两面OGS玻璃外形耐酸保护膜的周边形成凹槽;
3) 撕去基板表面的耐酸保护膜,对其进行钢化处理,钢化深度为0.010~0.015mm,形成母板;
4) 母板通过数道镀膜、黄光制程,在其一面凸起的区域形成图案及ITO线路,成为功能板,功能板有图案和ITO线路的一面作为OGS玻璃的功能感应面,另一面作为保护面;
5) 裁切去除功能板凹槽处连接玻璃,形成小片的OGS玻璃半成品;
6) 通过CNC对小片的OGS玻璃半成品裁切面进行打磨和抛光形成OGS玻璃成品。
本发明的优点在于,选用成本较低的大张OGS玻璃制造工艺,通过化学蚀刻后再钢化的方式,确保了OGS玻璃表面钢化层的完整性,从而满足了其应力层的完整性,保证了OGS产品强度及批量产品强度的一致性。
具体实施方式
以下结合实施例对本发明作进一步说明,OGS玻璃外形加工方法,其步骤如下:
1) 在大片玻璃正反两面印刷一一对应的OGS玻璃外形耐酸保护膜,耐酸保护膜尺寸比OGS玻璃外形尺寸单边大0.13mm~0.16mm;
2) 将大片玻璃浸泡在氰氟酸溶液中,进行等量蚀刻,氰氟酸浓度5%~30%(体积百分比),时间120min~150min,温度38℃~42℃,蚀刻深度为0.13mm~0.16mm,大张玻璃蚀刻后形成的基板正反两面OGS玻璃外形耐酸保护膜的周边形成凹槽;
3) 撕去基板表面的耐酸保护膜,对其进行钢化处理,钢化深度为0.010~0.015mm,形成母板;
4) 母板通过数道镀膜、黄光制程,在其一面凸起的区域形成图案及ITO线路,成为功能板,功能板有图案和ITO线路的一面作为OGS玻璃的功能感应面,另一面作为保护面;
5) 裁切去除功能板凹槽处连接玻璃,形成小片的OGS玻璃半成品;
6) 通过CNC对小片的OGS玻璃半成品裁切面进行打磨和抛光形成OGS玻璃成品。
实施例1:OGS玻璃外形加工方法,其步骤如下:
1)大张玻璃550mm×450mm×0.7mm,通过排版在正反面印刷8×5(横向8个,纵向5个)耐酸保护膜。耐酸保护膜上下一一对应。耐酸保护膜外形和OGS玻璃成品相同,尺寸单边比其大0.15mm。
2)将大片玻璃浸泡在氰氟酸溶液中,进行等量蚀刻,氰氟酸浓度20%(体积百分比),时间130min,温度40℃,蚀刻深度为0.15mm,蚀刻后的大张玻璃叫做基板,使基板的正反两面在OGS玻璃外形耐酸保护膜的周边形成凹槽。
3)撕去基板表面的耐酸保护膜,对其进行钢化处理,钢化深度为0.015mm,钢化后的基板叫做母板。
4)母板通过数道镀膜、黄光制程,在其一面凸起的区域形成图案及ITO线路,成为功能板,功能板有图案和ITO线路的一面作为OGS玻璃的感应面或功能面,另一面作为保护面。
5)裁切去除功能板凹槽处连接玻璃,形成小片的OGS玻璃半成品。
6)通过CNC对小片的OGS玻璃半成品裁切面进行打磨和抛光形成OGS玻璃成品。
实施例2:OGS玻璃外形加工方法,其步骤如下:
1)大张玻璃500mm×450mm×0.7mm,通过排版在正反面印刷7×4(横向7个,纵向4个)耐酸保护膜。耐酸保护膜上下一一对应。耐酸保护膜外形和OGS玻璃成品相同,尺寸单边比其大0.14mm。
2)将大片玻璃浸泡在氰氟酸溶液中,进行等量蚀刻,氰氟酸浓度10%(体积百分比),时间140min,温度38℃,蚀刻深度为0.14mm,蚀刻后的大张玻璃叫做基板,使基板的正反两面在OGS玻璃外形耐酸保护膜的周边形成凹槽。
3)撕去基板表面的耐酸保护膜,对其进行钢化处理,钢化深度为0.012mm,钢化后的基板叫做母板。
4)母板通过数道镀膜、黄光制程,在其一面凸起的区域形成图案及ITO线路,成为功能板,功能板有图案和ITO线路的一面作为OGS玻璃的感应面或功能面,另一面作为保护面。
5)裁切去除功能板凹槽处连接玻璃,形成小片的OGS玻璃半成品。
6)通过CNC对小片的OGS玻璃半成品裁切面进行打磨和抛光形成OGS玻璃成品。
本发明是将大片玻璃通过排版,在其正反两面印刷耐酸保护膜,保护膜外形比OGS玻璃外形单边大0.13mm~0.16mm,保护膜正反两面一一对应,形成多片OGS玻璃外形,然后将大片玻璃放入酸性溶液中进行等量的蚀刻,没有耐酸保护膜的区域将被蚀刻,蚀刻深度0.13mm~0.16mm。蚀刻后的大片玻璃叫基板,在基板的两面耐酸保护膜的四周将形成深0.13mm~0.16mm凹槽。撕掉基板正反两面的耐酸保护膜,对其进行物理钢化,钢化深度0.010~0.015mm。钢化后的基板叫母板。母板的表面有0.010~0.015mm的钢化层。再通过数道镀膜、黄光制程在母板的一面未被蚀刻的区域制作出图案和ITO线路,从而形成功能板。功能板通过裁切去掉凹槽部分的余料,形状小片的OGS玻璃半成品,最后过CNC打磨和抛光裁切面,形成OGS玻璃成品。

Claims (1)

1.OGS玻璃外形加工方法,其特征在于,其步骤如下:
1)在大片玻璃正反两面印刷一一对应的OGS玻璃外形耐酸保护膜,耐酸保护膜尺寸比OGS玻璃外形尺寸单边大0.13mm~0.16mm;
2)将大片玻璃浸泡在氰氟酸溶液中,进行等量蚀刻,氰氟酸浓度5%~30%,时间120min~150min,温度38℃~42℃,蚀刻深度为0.13mm~0.16mm,大张玻璃蚀刻后形成的基板正反两面OGS玻璃外形耐酸保护膜的周边形成凹槽;
3)撕去基板表面的耐酸保护膜,对其进行钢化处理,钢化深度为0.010~0.015mm,形成母板;
4)母板通过数道镀膜、黄光制程,在其一面凸起的区域形成图案及ITO线路,成为功能板,功能板有图案和ITO线路的一面作为OGS玻璃的功能感应面,另一面作为保护面;
5)裁切去除功能板凹槽处连接玻璃,形成小片的OGS玻璃半成品;
6)通过CNC对小片的OGS玻璃半成品裁切面进行打磨和抛光形成OGS玻璃成品。
CN201210542906.7A 2012-12-15 2012-12-15 Ogs玻璃的外形加工方法 Active CN102999240B (zh)