CN1020468C - 难成浆煤用沥青作添加剂配制高浓度水煤浆 - Google Patents

难成浆煤用沥青作添加剂配制高浓度水煤浆 Download PDF

Info

Publication number
CN1020468C
CN1020468C CN 87102923 CN87102923A CN1020468C CN 1020468 C CN1020468 C CN 1020468C CN 87102923 CN87102923 CN 87102923 CN 87102923 A CN87102923 A CN 87102923A CN 1020468 C CN1020468 C CN 1020468C
Authority
CN
China
Prior art keywords
coal
pitch
water
additive
slurry
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 87102923
Other languages
English (en)
Other versions
CN87102923A (zh
Inventor
臧子秀
江龙
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Institute of Photographic Chemistry of CAS
Original Assignee
Institute of Photographic Chemistry of CAS
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Institute of Photographic Chemistry of CAS filed Critical Institute of Photographic Chemistry of CAS
Priority to CN 87102923 priority Critical patent/CN1020468C/zh
Publication of CN87102923A publication Critical patent/CN87102923A/zh
Application granted granted Critical
Publication of CN1020468C publication Critical patent/CN1020468C/zh
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

本发明是关于在难成浆的煤的粉碎及细磨过程中,加入表面处理添加剂沥青,改变了煤本身的亲水性,改善了煤的成浆性,在不增加水煤浆粘度的情况下,提高了水煤浆中煤的固体含量。而沥青来源广泛,价格低廉,是一种理想的表面处理添加剂。

Description

本发明属于一种新型液体燃料水煤浆。
随着水煤浆制备技术走向工业化,人们对煤的研究也逐步深入,在制备水煤浆时,煤的品种起着十分重要的作用,Watanabe等实验证明,煤中所含灰份对煤的成浆性能是有影响的[第六届国际煤浆会议(1984)]。王祖纳、张荣曾等指出煤的内含水量愈高,则愈不易成浆[第八届国际煤浆及制备会议(1986)],吴家珊等证明(燃料化学学报)煤的含氧基团愈多,则愈不易成浆,以上这些工作证明,煤的表面亲水性愈高,则愈不易形成粘度小的水煤浆,以上这些工作都说明了煤的表面性质对水煤浆的成浆性质有十分重要的作用。
梁文平等使用了溴化十六吡啶作为煤的表面处理添加剂,使煤的表面疏水,可以提高煤的成浆性。指出了改善煤的成浆性的方向,但这类阳离子表面活性剂成本昂贵,而且改善煤的成浆效果不明显,因而这类表面处理添加剂没有工业应用价值。
在我国,有不少地方有优质煤,例如柠条塔矿的神木煤,灰分低,挥发分高,虽然是理想的制备水煤浆的原料,但其成浆性能太差,难以制备高浓度的水煤浆,如果找到一种价廉而高效的表面处理添加剂,这对于扩大水煤浆的煤种,使之用于制备水煤浆,便具有十分重要的意义。
本发明的目的是使用沥青作为表面处理添加剂,在煤粉碎和研磨过程中,把沥青加入到难成浆的煤中,沥青加入量为煤的干基重量的0.5-10%,可以明显地降低水煤浆的粘度,表1比较了在相同浓度下(70%煤干基含量)加沥青和不加沥青各种煤制备水煤浆的粘 度差异。
表1
煤种    粘度(厘泊)    未加沥青    加沥青
柠条塔    1080    476
府各    2088    1428
左云    1068    652
恩口    528    532
注:1、粘度测量用NDJ-1型粘度计测定(上海天平仪器厂出品)
2、煤粉粒度60%的煤粉颗粒小于200目,最大颗粒不超过250μ
3、沥青与煤粉的比例0.5-10∶99.5-90各种添加剂与煤的用量比<2%
从表1的数据可以看到,加沥青后对柠条塔煤、府各煤、左云煤都大大降低了用他们制备的水煤浆的粘度。而对恩口煤是例外,我们又测定了煤的润湿角,对比数据是加沥青和不加沥青的,结果见表2,从表2数据可以证明,加入沥青提高了煤的疏水性,因而降低了水煤浆的粘度,而恩口煤本身就具有较高的疏水性,因此加入沥青后,粘度不会有改变。
表2
煤种    润湿角α°    未加沥青    加沥青
柠条塔    16.5    46.5
府各    10    50.2
左云    8    39.8
恩口    62.8    60.9
沥青    65.5
沥青来源广泛,价格便宜,大量用于建筑和铺路的防水材料,它的灰分只占百分之零点几。而挥发份大于50%,用于制备水煤浆降低粘度效果明显,并有帮助燃烧和提高煤浆稳定性的特点,是一种理想的工业表面处理添加剂,使用它不会增加水煤浆的成本。各种沥青包括煤焦油沥青、石油沥青和电极沥青都可以用在本发明专利中作表面处理添加剂。
本发明的实施例一
煤种:神木煤(柠条塔矿)
煤粉粒度:60目~200目    30%
200目以下    70%
在相同粘度条件下,由于加入沥青使制得的水煤浆浓度增大,结果见表3、表4。
表3
添加剂用量    水煤浆浓度    粘度
添加剂种类    (占煤干基含量    (煤干基含量%)    (厘泊)
%)
萘磺酸甲醛    1    68.8    1200
缩合物
磺化腐植酸    1    67.1    1200
木质素磺酸钙    1.5    65    1200
表4
添加剂用量    沥青用量占    水煤浆浓度(煤    粘度
添加剂种类    (占煤干基含    煤干基%    干基含量%)    (厘泊)
量%)
萘磺酸甲醛    1    2    71.5    1200
缩合物
磺化腐植酸    1    2    69.8    1200
木质素磺酸钙    1.5    2    67.6    1200
本发明实施例二
煤种:山西左云煤
煤粉粒度:200目以下占80%,单蝉浆在相同粘度条件下,由于加入沥青使制得的水煤浆浓度增大,结果见表5、表6。
表5
添加剂用量占煤    水煤浆浓度占煤    粘度
添加剂种类    干基含量%    干基含量%    (厘泊)
萘磺酸甲醛    1    61.2    1000
缩合物
磺化腐植酸    1    58.2    1000
木质素磺酸钙    1.5    56    1000
表6
添加剂用量    沥青用量(占    水煤浆浓度(占    粘度
添加剂种类    (占煤干基含    煤干基%)    煤干基含量%)    (厘泊)
萘磺酸甲醛    1    2.5    63.9    1000
缩合物
磺化腐植酸    1    2.5    60.1    1000
木质素磺酸钙    1.5    2.5    58.4    1000

Claims (3)

1、一种由难成浆煤、水以及添加剂组成的高浓度水煤浆,其特征在于在难成浆的煤粉碎过程中把沥青作表面处理添加剂加入到难成浆的煤中,沥青用量为煤的(千重)0.5-10%。
2、如权利要求1所说的水煤浆,其特征在于表面处理剂沥青包括煤焦油沥青,石油沥青和电极用沥青。
3、根据权利要求1,2所说的水煤浆,其特征在于水煤浆的浓度为60-72%。
CN 87102923 1987-04-23 1987-04-23 难成浆煤用沥青作添加剂配制高浓度水煤浆 Expired - Fee Related CN1020468C (zh)