CN101774068B - 不锈钢复合钢板埋弧焊焊接工艺 - Google Patents

不锈钢复合钢板埋弧焊焊接工艺 Download PDF

Info

Publication number
CN101774068B
CN101774068B CN2009102564084A CN200910256408A CN101774068B CN 101774068 B CN101774068 B CN 101774068B CN 2009102564084 A CN2009102564084 A CN 2009102564084A CN 200910256408 A CN200910256408 A CN 200910256408A CN 101774068 B CN101774068 B CN 101774068B
Authority
CN
China
Prior art keywords
welding
steel plate
basic unit
groove
weld seam
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN2009102564084A
Other languages
English (en)
Other versions
CN101774068A (zh
Inventor
黄孝鹏
高希改
崔昌宇
吴海伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Luxi Industrial Equipment Co Ltd
Original Assignee
Luxi Industrial Equipment Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Luxi Industrial Equipment Co Ltd filed Critical Luxi Industrial Equipment Co Ltd
Priority to CN2009102564084A priority Critical patent/CN101774068B/zh
Publication of CN101774068A publication Critical patent/CN101774068A/zh
Application granted granted Critical
Publication of CN101774068B publication Critical patent/CN101774068B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种不锈钢复合钢板埋弧焊焊接工艺。它可有效降低焊工劳动强度、提高劳动条件、生产效率和焊缝质量,降低生产成本等优点,其工艺为:1)加工坡口,将待焊接的不锈钢复合钢板的焊接端处理成坡口;2)以坡口中部焊道为基层打底焊缝,以基层打底焊缝上部临近不锈钢复合钢板复合层的焊道为复层焊缝,以基层打底焊缝下部焊道为基层填充盖面焊缝;3)对于基层打底焊缝采用传统工艺焊接;4)对于基层填充盖面焊缝采用传统工艺焊接;5)对于复层焊缝焊接时,焊接电流为350-400A,焊接电压为28-30V,焊接速度为40-50cm/min。

Description

不锈钢复合钢板埋弧焊焊接工艺
技术领域
本发明涉及一种埋弧焊焊接工艺,尤其涉及一种不锈钢复合钢板过渡层和复层焊接用不锈钢复合钢板埋弧焊焊接工艺。
背景技术
在传统不锈钢复合钢板(碳素钢、低合金钢+0Cr18Ni9)过渡层和复层的焊接时,为减少基层对过渡层的稀释,防止接头产生马氏体组织,出现裂纹缺陷,往往过渡层采用高铬镍的抗稀释性好的双相铬镍不锈钢焊条进行手工电弧焊焊接。但手工电弧焊操作工人的劳动条件差,劳动强度大。由于焊条的长度有限,不能连续焊接,所以生产效率较低,并且焊缝的质量取决于焊工的操作技能水平。
发明内容
本发明的目的就是为了解决上述问题,提供一种可有效降低焊工劳动强度、提高劳动条件、生产效率和焊缝质量,降低生产成本等优点的不锈钢复合钢板埋弧焊焊接工艺。
为实现上述目的,本发明采用如下技术方案:
一种不锈钢复合钢板埋弧焊焊接工艺,它的步骤为:
1)加工坡口,将待焊接的不锈钢复合钢板的焊接端处理成坡口;
2)以坡口中部焊道为基层打底焊缝,以基层打底焊缝上部临近不锈钢复合钢板复合层的焊道为复层焊缝,以基层打底焊缝下部焊道为基层填充盖面焊缝;
3)对于基层打底焊缝采用传统工艺焊接;
4)对于基层填充盖面焊缝采用传统工艺焊接;
5)对于复层焊缝焊接时,焊接电流为350-400A,焊接电压为28-30V,焊接速度为40-50cm/min。
所述步骤1)中,坡口的中部宽度为2±1mm或6±1mm,两相对不锈钢复合钢板坡口间夹角为65°±5°,两相对不锈钢复合钢板坡口中部间隙为1±1mm,坡口距不锈钢复合钢板复合层表面距离为9±1mm或12±1mm,不锈钢复合钢板厚度为18-40mm。
所述基层打底焊缝上表面距不锈钢复合钢板复合层下表面3.0-4.5mm。
本发明的有益效果是:焊接工艺通过改变坡口形式、焊道分布以及调整工艺参数,采用埋弧自动焊,达到降低焊工劳动强度、提高劳动条件、生产效率和焊缝质量,降低生产成本的目的。
附图说明
图1为坡口结构示意图;
图2为焊道分布结构示意图。
其中,1.不锈钢复合钢板,2.复合层,3.坡口,4.基层打底焊缝,5.基层填充盖面焊缝,6.复层焊缝。
具体实施方式
下面结合附图与实施例对本发明做进一步说明。
本发明的工艺为:
1)加工坡口3,将待焊接的不锈钢复合钢板1的焊接端处理成坡口3;坡口3可适用于平板对接,筒体纵、环缝。坡口的中部宽度为2±1mm或6±1mm,两相对不锈钢复合钢板坡口间夹角为65°±5°,两相对不锈钢复合钢板坡口中部间隙为1±1mm,坡口距不锈钢复合钢板复合层表面距离为9±1mm或12±1mm,不锈钢复合钢板厚度为18-40mm。见图1。
2)以坡口3中部焊道为基层打底焊缝4,以基层打底焊缝4上部临近不锈钢复合钢板复合层2的焊道为复层焊缝6,以基层打底焊缝4下部焊道为基层填充盖面焊缝5;基层打底焊缝上表面距不锈钢复合钢板复合层下表面3.0-4.5mm。见图2。
3)对于基层打底焊缝4采用传统工艺焊接;见表1
4)对于基层填充盖面焊缝5采用传统工艺焊接;见表1
5)对于复层焊缝6焊接时,焊接电流为350-400A,焊接电压为28-30V,焊接速度为40-50cm/min。见表1。
表1焊接工艺参数
Figure G2009102564084D00021

Claims (1)

1.一种不锈钢复合钢板埋弧焊焊接工艺,其特征是,它的步骤为:
1)加工坡口,将待焊接的不锈钢复合钢板的焊接端处理成坡口;
2)以坡口中部焊道为基层打底焊缝,以基层打底焊缝上部临近不锈钢复合钢板复合层的焊道为复层焊缝,以基层打底焊缝下部焊道为基层填充盖面焊缝;
3)对于基层打底焊缝采用传统工艺焊接;
4)对于基层填充盖面焊缝采用传统工艺焊接;
5)对于复层焊缝焊接时,焊接电流为350-400A,焊接电压为28-30V,焊接速度为40-50cm/min;
所述步骤1)中,坡口的中部宽度为2±1mm或6±1mm,两相对不锈钢复合钢板坡口间夹角为65°±5°,两相对不锈钢复合钢板坡口中部间隙为1±1mm,坡口距不锈钢复合钢板复合层表面距离为9±1mm或12±1mm,不锈钢复合钢板厚度为18-40mm,
所述基层打底焊缝上表面距不锈钢复合钢板复合层下表面3.0-4.5mm。 
CN2009102564084A 2009-12-25 2009-12-25 不锈钢复合钢板埋弧焊焊接工艺 Active CN101774068B (zh)