CN101468581B - 家具硝基仿古涂装古树皮效果装饰的施工工艺 - Google Patents

家具硝基仿古涂装古树皮效果装饰的施工工艺 Download PDF

Info

Publication number
CN101468581B
CN101468581B CN 200710173773 CN200710173773A CN101468581B CN 101468581 B CN101468581 B CN 101468581B CN 200710173773 CN200710173773 CN 200710173773 CN 200710173773 A CN200710173773 A CN 200710173773A CN 101468581 B CN101468581 B CN 101468581B
Authority
CN
China
Prior art keywords
nitro
nitryl
primer
dry
coated
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN 200710173773
Other languages
English (en)
Other versions
CN101468581A (zh
Inventor
钟华胜
刘林生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHANGHAI ZHANCHEN PAINT Co.,Ltd.
Zhuhai zhanchen New Material Co., Ltd
Original Assignee
Shanghai Fuchen Chemical Co Ltd
Beijing Zhanchen Chemical Co Ltd
Zhanchen Paint Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shanghai Fuchen Chemical Co Ltd, Beijing Zhanchen Chemical Co Ltd, Zhanchen Paint Group Co Ltd filed Critical Shanghai Fuchen Chemical Co Ltd
Priority to CN 200710173773 priority Critical patent/CN101468581B/zh
Publication of CN101468581A publication Critical patent/CN101468581A/zh
Application granted granted Critical
Publication of CN101468581B publication Critical patent/CN101468581B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及家居装饰技术领域,具体涉及一种家具硝基仿古涂装古树皮效果装饰施工工艺。本发明公开了一种家具硝基仿古涂装古树皮效果装饰施工工艺包括下列步骤:素材砂光,聚氨脂透明底漆喷涂,聚氨脂透明底漆砂光,聚氨酯浅黄底漆喷涂,刷涂硝基透明底漆,刷涂硝基裂纹漆,脱落处理,硝基透明底漆喷涂,硝基透明底漆砂光,)裂纹漆处布印,硝基格丽斯干刷,硝基透明底漆喷涂,硝基透明底漆砂光,喷点,硝基底漆喷涂,灰尘漆,硝基透明面漆喷涂。本发明的工艺可以在中纤板或其它复合材料上达到一种仿古树皮的涂装装饰效果,可以不采用实木木材也能达到一种古树皮的仿古效果,从而可以满足有关人员的需求。

Description

家具硝基仿古涂装古树皮效果装饰的施工工艺
技术领域
本发明涉及家居装饰技术领域,具体涉及一种家具硝基仿古涂装古树皮效果装饰施工工艺。
背景技术
同时随着我国经济的飞速发展,家居家具制品消费的日趋旺盛,目前市场上大部分家具都是实木制作,加剧森林的砍伐,造成生态环境的破坏和资源紧缺,人们在生产加工逐渐用密度板或其它复合材料来替代实木,而这些材料的涂装效果无法达到实木的效果,工艺相对比较单一,大多采用的是实色或珠光漆涂装的镜面效果,不能满足消费者的需求。
因此,急需开发家具仿古树皮装饰效果的施工艺能够填补这方面的不足,满足消费者的需求。
发明内容
本发明所要解决的问题为家具仿古树皮装饰方面的工艺问题,以使家具既能被赋予仿古树皮效果,同时又能保障仿古家具表面涂层的质量和外观。
本发明为了解决上述问题,公开了一种家具硝基仿古涂装古树皮效果装饰施工工艺,包括下列步骤:
a)素材砂光:用砂纸顺木纹砂磨,去除素材表面毛刺、砂痕;
b)涂聚氨酯底漆:用聚氨酯底漆配固化剂,再加入聚氨酯稀释剂调至粘度13~14秒,人工喷涂一个“十”字,干燥2~3小时;
c)砂光:用砂纸砂磨平整、光滑;
d)涂聚氨酯浅黄底漆:用调配好颜色的浅黄底漆配固化剂,再加入聚氨酯稀释剂调至粘度14~15秒,人工喷涂一个“十”字,干燥12小时以上;
e)涂硝基透明底漆:用毛刷沾高粘度的硝基透明底漆不规则局部人工刷涂,达到自然效果,干燥3~4小时;
f)涂硝基裂纹漆:用调配好颜色的硝基裂纹漆按配比调至粘度14~15秒,人工厚薄不一刷涂于表面,干燥6~8小时;
g)脱落处理:用百洁布把无附着力的裂纹漆擦去除,达到自然的脱落效果;
h)涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度12~13秒,人工喷涂一个“十”字,干燥20~30分钟,然后再做二次喷涂,干燥50~60分钟;
i)砂光:用600#砂纸轻砂,去除表面颗粒;
j)裂纹漆处布印:用棉碎布沾调好颜色的布印着色剂,不规则重复拍打在裂纹漆表面,拍打时注意保持深浅不一,使其达到自然的效果;
k)干刷:用毛刷沾调配好颜色的硝基格丽斯拍打表面,裂纹漆表面略为要深些,沟槽部分略浅,使其达到深浅不一的自然效果;
l)涂硝基透明底漆:用硝基透明底漆呈“十字”方式均匀喷涂于素材表面,干燥60~80分钟;
m)砂光:用600#砂纸轻砂表面,无颗粒;
n)喷点:用调配好颜色的喷点,用喷枪在适量气压下人工喷涂表面,使其达到陈旧效果;
o)涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度14~15秒,人工均匀喷涂一个“十”字,干燥60~80分钟;
p)灰尘漆:用布沾调配好颜色的灰尘漆抹涂在裂纹漆部分,达到自然效果;
q)硝基透明面漆:用硝基透明面漆冲配硝基稀释剂调至粘度12~13秒,喷涂一个“十”字,干燥36小时即可。
本发明中,步骤a)中所述砂纸优选240#砂纸,以便在用砂纸顺木纹砂磨时,能短时间内高效地去除素材表面毛刺、砂痕等。
所述的粘度均为岩田-2#杯粘度。
所述的素材为室内家居产品,如中纤板或其它复合材料组成的家具产品。
所述的硝基稀释剂为二甲苯、乙二醇单丁醚、乙酸丁酯或它们组成的混合溶剂。
术语“布印、明暗、干刷”均为本领域公知的术语,在美式仿古涂装工艺记录中上有详细的描述。
本发明的工艺可以在中纤板或其它复合材料上达到一种仿古树皮的涂装装饰效果,可以不采用实木木材也能达到一种古树皮的仿古效果。
具体实施方式
以下结合具体实施例,进一步阐明本发明。应理解,这些实施例仅用于说明本发明而不用于限制本发明的范围。下列实施例中未注明具体条件的实验方法,通常按照常规条件,或按照制造厂商所建议的条件。比例和百分比基于重量,除非特别说明。
实施例1制备拉丝仿古涂装效果的中纤板
中纤板砂光:用240#砂纸顺木纹砂磨,去除中纤板表面毛刺、砂痕等;涂聚氨酯透明底漆:用聚氨酯底漆配固化剂,再加入适量聚氨酯稀释剂调至粘度13~14秒,人工喷涂一个“十”字,干燥2~3小时;砂光:用400#砂纸砂磨平整、光滑;涂聚氨酯浅黄底漆:用调配好颜色的浅黄底漆配固化剂,再加入适量聚氨酯稀释剂调至粘度14~15秒,人工喷涂一个“十”字,干燥12小时以上;刷涂硝基透明底漆:用毛刷沾高粘度的硝基透明底漆不规则局部人工刷涂,达到自然效果,干燥3~4小时;涂硝基裂纹漆:用调配好颜色的硝基裂纹漆按配比调至粘度14~15秒,人工厚薄不一刷涂于表面,干燥6~8小时;脱落处理:用百洁布把无附着力的裂纹漆擦去除,达到自然的脱落效果;涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度12~13秒,人工喷涂一个“十”字,干燥20~30分钟,然后再做二次喷涂,干燥50~60分钟;砂光:用600#砂纸轻砂,去除表面颗粒;裂纹漆处布印:用棉碎布沾调好颜色的布印着色剂,不规则重复拍打在裂纹漆表面,拍打时注意保持深浅不一,使其达到自然的效果;干刷:用毛刷沾调配好颜色的硝基格丽斯拍打表面,裂纹漆表面略为要深些,沟槽部分略浅,使其达到深浅不一的自然效果;涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度14~15秒,人工均匀喷涂一个“十”字,干燥60~80分钟;砂光:用600#砂纸轻砂表面,无颗粒;喷点:用调配好颜色的喷点,用喷枪人工喷涂表面,使其达到陈旧效果;涂硝基底漆:用硝基透明底漆加入硝基稀释剂调配至粘度14~15秒,人工均匀喷涂一个“十”字,干燥60~80分钟;灰尘漆:用布沾适量调配好颜色的灰尘漆抹涂在裂纹漆部分,达到自然效果;硝基透明面漆:用硝基透明面漆冲配硝基稀释剂调至粘度12~13秒,喷涂一个“十”字,干燥36小时即可得仿古树皮的装饰效果效果的中纤板。
本发明的范围不受所述具体实施方案的限制,所述实施方案只欲作为阐明本发明各个方面的单个例子,本发明范围内还包括功能等同的方法和组分。实际上,除了本文所述的内容外,本领域技术人员参照上文的描述和附图可以容易地掌握对本发明的多种改进。所述改进也落入所附权利要求书的范围之内。上文提及的每篇参考文献皆全文列入本文作为参考。

Claims (5)

1.一种家具硝基仿古涂装古树皮效果装饰施工工艺,包括下列步骤:
a)素材砂光:用砂纸顺木纹砂磨,去除素材表面毛刺、砂痕;
b)涂聚氨酯底漆:用聚氨酯底漆配固化剂,再加入聚氨酯稀释剂调至粘度13~14秒,人工喷涂一个“十”字,干燥2~3小时;
c)砂光:用砂纸砂磨平整、光滑;
d)涂聚氨酯浅黄底漆:用调配好颜色的浅黄底漆配固化剂,再加入聚氨酯稀释剂调至粘度14~15秒,人工喷涂一个“十”字,干燥12小时以上;
e)涂硝基透明底漆:用毛刷沾高粘度的硝基透明底漆不规则局部人工刷涂,达到自然效果,干燥3~4小时;
f)涂硝基裂纹漆:用调配好颜色的硝基裂纹漆按配比调至粘度14~15秒,人工厚薄不一刷涂于表面,干燥6~8小时;
g)脱落处理:用百洁布把无附着力的裂纹漆擦去除,达到自然的脱落效果;
h)涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度12~13秒,人工喷涂一个“十”字,干燥20~30分钟,然后再做二次喷涂,干燥50~60分钟;
i)砂光:用600#砂纸轻砂,去除表面颗粒;
j)裂纹漆处布印:用棉碎布沾调好颜色的布印着色剂,不规则重复拍打在裂纹漆表面,拍打时注意保持深浅不一,使其达到自然的效果; 
k)干刷:用毛刷沾调配好颜色的硝基格丽斯拍打表面,裂纹漆表面略为要深些,沟槽部分略浅,使其达到深浅不一的自然效果;
l)涂硝基透明底漆:用硝基透明底漆呈“十字”方式均匀喷涂于素材表面,干燥60~80分钟;
m)砂光:用600#砂纸轻砂表面,无颗粒;
n)喷点:用调配好颜色的喷点,用喷枪在适量气压下人工喷涂表面,使其达到陈旧效果;
o)涂硝基透明底漆:用硝基透明底漆加入硝基稀释剂调配至粘度14~15秒,人工均匀喷涂一个“十”字,干燥60~80分钟;
p)灰尘漆:用布沾调配好颜色的灰尘漆抹涂在裂纹漆部分,达到自然效果;
q)硝基透明面漆:用硝基透明面漆冲配硝基稀释剂调至粘度12~13秒,喷涂一个“十”字,干燥36小时即可;
所述的粘度均为岩田-2#杯粘度。
2.根据权利要求1所述的施工工艺,其特征在于所述步骤a)中所述砂纸为240#砂纸。
3.根据权利要求1或2所述的施工工艺,其特征在于所述硝基稀释剂为二甲苯、乙二醇单丁醚、乙酸丁酯或它们组成的混合溶剂。
4.根据权利要求1所述的施工工艺,其特征在于所述素材为室内家居产品。
5.根据权利要求4所述的施工工艺,其特征在于所述室内家居产品的材质为中纤板或其它复合材料。 
CN 200710173773 2007-12-29 2007-12-29 家具硝基仿古涂装古树皮效果装饰的施工工艺 Active CN101468581B (zh)