WO2024225472A1 - 光学積層体及びこれを備えた物品 - Google Patents

光学積層体及びこれを備えた物品 Download PDF

Info

Publication number
WO2024225472A1
WO2024225472A1 PCT/JP2024/016571 JP2024016571W WO2024225472A1 WO 2024225472 A1 WO2024225472 A1 WO 2024225472A1 JP 2024016571 W JP2024016571 W JP 2024016571W WO 2024225472 A1 WO2024225472 A1 WO 2024225472A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
optical laminate
optical
hard coat
refractive index
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2024/016571
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
尚太郎 源田
昇平 吉田
猛 厳
直樹 薄井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dexerials Corp
Original Assignee
Dexerials Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dexerials Corp filed Critical Dexerials Corp
Priority to CN202480026779.6A priority Critical patent/CN121002404A/zh
Priority to KR1020257034507A priority patent/KR20250168355A/ko
Publication of WO2024225472A1 publication Critical patent/WO2024225472A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B32B27/18—Layered products comprising a layer of synthetic resin characterised by the use of special additives
    • B32B27/20—Layered products comprising a layer of synthetic resin characterised by the use of special additives using fillers, pigments, thixotroping agents
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
    • B32B7/02—Physical, chemical or physicochemical properties
    • B32B7/023—Optical properties
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/11—Anti-reflection coatings
    • G02B1/113—Anti-reflection coatings using inorganic layer materials only
    • G02B1/115—Multilayers
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/14—Protective coatings, e.g. hard coatings
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/18—Coatings for keeping optical surfaces clean, e.g. hydrophobic or photo-catalytic films

Definitions

  • the present invention relates to an optical laminate and an article including the same, and in particular to an optical laminate used as an anti-reflection film suitable for displays that are used in a bent state, such as flexible displays, and an article including the same.
  • This application claims priority based on Japanese Patent Application No. 2023-074698 filed in Japan on April 28, 2023, Japanese Patent Application No. 2024-063462 filed in Japan on April 10, 2024, and Japanese Patent Application No. 2024-069031 filed in Japan on April 22, 2024, the contents of which are incorporated herein by reference.
  • optical laminates such as anti-reflection films are sometimes used to reduce surface reflection.
  • Optical laminates used in foldable displays are subject to higher demands for durability against bending than non-foldable displays.
  • Patent Document 1 proposes improving the bending resistance of a hard coat film having a hard coat layer and an optical functional layer made of a sputtered film by setting the thickness ratio of the hard coat layer to the optical functional layer within a specified range.
  • Patent Document 2 also describes how bending resistance can be improved by making the hard coat layer and anti-reflection layer out of resin.
  • Patent Document 1 aims to improve the abrasion resistance and bending resistance of the hard coat film, it does not evaluate the scratch resistance, and there is room for improvement.
  • the anti-reflection film in Patent Document 2 can improve the bending resistance, the anti-reflection layer is made of resin, and therefore the scratch resistance is poor.
  • the present invention was made in consideration of the above problems, and aims to provide an optical laminate that can achieve excellent scratch resistance and further improves bending resistance, and an article including the same.
  • An optical laminate having, in this order, a transparent substrate, a hard coat layer, an adhesion layer made of a sputtered film, a high refractive index layer made of a sputtered film, and an optical functional layer in which a low refractive index layer having a refractive index lower than that of the high refractive index layer is alternately laminated, and an antifouling layer,
  • the hard coat layer contains a silica filler
  • Condition 1 The ratio ((A)/(B)) of the Martens hardness (A) measured from the antifouling layer side of the optical laminate to the Martens hardness (B) measured from the hard coat layer side of a laminate having only the transparent substrate and the hard coat layer is 3.6 or less.
  • Condition 2 Using a friction tester using steel wool conforming to JIS L0849, the steel wool is horizontally reciprocated 200 times, and the difference in contact angle with water before and after friction is 20° or less.
  • silane compound is one or more selected from a vinyl group-containing silane compound, a (meth)acryloyl group-containing silane compound, an amino group-containing silane compound, an isocyanate group-containing silane compound, an isocyanurate group-containing silane compound, an epoxy group-containing silane compound, and a mercapto group-containing silane compound.
  • the hard coat layer contains a binder resin and a silica filler,
  • the binder resin contains a (meth)acrylate compound, The optical laminate according to the above-mentioned [5], wherein the functional group derived from the silane compound is a (meth)acryloyl group.
  • the present invention makes it possible to provide an optical laminate that has excellent scratch resistance and further improved bending resistance, and an article that includes the same.
  • FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment.
  • FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment.
  • FIG. 2 is a schematic diagram for explaining an example of a manufacturing apparatus that can be used in the manufacturing method of the optical laminate of the present embodiment.
  • FIG. 1 is a cross-sectional view showing another example of the optical laminate of the present embodiment.
  • the optical laminate 102 shown in FIG. 1 is formed by laminating a transparent substrate 11, a hard coat layer 12, an adhesive layer 13, an optically functional layer 14, and an antifouling layer 15 in this order.
  • the adhesion layer 13 is a layer that provides adhesion between the hard coat layer 12 and the optical function layer 14 .
  • the optical function layer 14 is a layer that exhibits an optical function.
  • the optical function is a function that controls the properties of light, such as reflection, transmission, and refraction, and examples of the optical function include an anti-reflection function, a selective reflection function, and a lens function.
  • the optical functional layer 14 preferably includes any one selected from an antireflection layer and a selective reflection layer.
  • an antireflection layer and a selective reflection layer known layers can be used.
  • Each of the antireflection layer and the selective reflection layer may be a single layer or a laminate of multiple layers.
  • FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment.
  • the optical laminate 101 shown in Fig. 2 is provided with an antireflection layer as the optical functional layer 14 in the optical laminate 102 shown in Fig. 1.
  • the optical functional layer 14 (antireflection layer) is made of a laminate in which low refractive index layers 14b and high refractive index layers 14a are alternately laminated as shown in Fig. 1.
  • the antifouling layer 15 is in contact with the low refractive index layer 14b of the optical functional layer 14.
  • the transparent substrate 11 may be formed from a transparent material capable of transmitting light in the visible light range.
  • a plastic film is preferably used as the transparent substrate 11.
  • materials constituting the plastic film include polyester-based resins, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, and polyphenylene sulfide-based resins.
  • the term "transparent material” refers to a material having a transmittance of 80% or more for light in the wavelength range used, provided that the effect of the present invention is not impaired.
  • (meth)acrylic means methacryl and acrylic.
  • the transparent substrate 11 may contain a reinforcing material as long as the optical properties are not significantly impaired.
  • the reinforcing material include cellulose nanofiber and nanosilica.
  • polyester-based resins, acetate-based resins, polycarbonate-based resins, and polyolefin-based resins are preferably used as the reinforcing material.
  • a triacetyl cellulose (TAC) substrate is preferably used as the reinforcing material.
  • the transparent substrate 11 may also be a glass film, which is an inorganic substrate.
  • the plastic film is a TAC substrate
  • a hard coat layer 12 is formed on one side of the substrate
  • a permeation layer is formed in which some of the components that make up the hard coat layer 12 penetrate.
  • the adhesion between the transparent substrate 11 and the hard coat layer 12 is improved, and the occurrence of interference fringes due to the difference in refractive index between the layers can be suppressed.
  • the transparent substrate 11 may be a film that has optical and/or physical functions.
  • films that have optical and/or physical functions include polarizing plates, phase difference compensation films, heat-blocking films, transparent conductive films, brightness-enhancing films, and barrier-enhancing films.
  • the thickness of the transparent substrate 11 is not particularly limited, but is preferably, for example, 25 ⁇ m or more, and more preferably, 40 ⁇ m or more.
  • the thickness of the transparent substrate 11 is 25 ⁇ m or more, the rigidity of the substrate itself is ensured, and wrinkles are unlikely to occur even when stress is applied to the optical laminate 10.
  • the thickness of the transparent substrate 11 is 25 ⁇ m or more, wrinkles are unlikely to occur even when the hard coat layer 12 is continuously formed on the transparent substrate 11, and there are fewer manufacturing concerns, which is preferable.
  • the thickness of the transparent substrate 11 is 40 ⁇ m or more, wrinkles are even less likely to occur, which is preferable.
  • the thickness of the transparent substrate 11 is preferably 1000 ⁇ m or less, and more preferably 600 ⁇ m or less.
  • the optical laminate 10 during manufacturing and the optical laminate 10 after manufacturing can be easily wound into a roll, and the optical laminate 10 can be manufactured efficiently.
  • the optical laminate 10 can be made thinner and lighter.
  • the optical laminate 10 can be manufactured more efficiently and can be made even thinner and lighter, which is preferable.
  • the surface of the transparent substrate 11 may be previously subjected to an etching treatment such as sputtering, corona discharge, ultraviolet irradiation, electron beam irradiation, conversion, oxidation, and/or an undercoat treatment. By previously performing these treatments, it is possible to improve adhesion with the hard coat layer 12 formed on the transparent substrate 11. In addition, it is also preferable to remove dust and clean the surface of the transparent substrate 11 by performing solvent washing, ultrasonic washing, etc. on the surface of the transparent substrate 11 before forming the hard coat layer 12 on the transparent substrate 11, as necessary.
  • an etching treatment such as sputtering, corona discharge, ultraviolet irradiation, electron beam irradiation, conversion, oxidation, and/or an undercoat treatment.
  • the hard coat layer 12 contains a binder resin and a filler as essential components, and may contain other components such as a dispersant as optional components.
  • a known binder resin can be used.
  • the filler is contained in the binder resin to the extent that the transparency is not impaired.
  • the filler may be made of an organic material, an inorganic material, or a combination of an organic material and an inorganic material, but from the viewpoint of hardness and flex resistance, an inorganic material is preferred, silica particles made of silica are more preferred, and surface-modified silica particles are particularly preferred.
  • the binder resin used in the hard coat layer 12 is preferably transparent, and examples of resins that can be used include ionizing radiation curable resins that are cured by ultraviolet light or electron beams, thermoplastic resins, and thermosetting resins.
  • Examples of the ionizing radiation curable resin used as the binder resin of the hard coat layer 12 include ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone.
  • Examples of the compound that is an ionizing radiation curable resin having two or more unsaturated bonds include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane ...
  • polyfunctional compounds examples include erythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate.
  • pentaerythritol triacrylate PETA
  • dipentaerythritol hexaacrylate DPHA
  • pentaerythritol tetraacrylate PETA
  • (meth)acrylate refers to methacrylate and acrylate.
  • the above-mentioned compounds modified with PO (propylene oxide), EO (ethylene oxide), CL (caprolactone), etc. can also be used.
  • urethane (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, etc. can also be used from the viewpoint of film formation of the hard coat layer and adjustment of viscoelasticity.
  • Thermoplastic resins used as the binder resin of the hard coat layer 12 include, for example, styrene-based resins, (meth)acrylic resins, vinyl acetate-based resins, vinyl ether-based resins, halogen-containing resins, alicyclic olefin-based resins, polycarbonate-based resins, polyester-based resins, polyamide-based resins, cellulose derivatives, silicone-based resins, and rubber or elastomers.
  • the above-mentioned thermoplastic resins are preferably non-crystalline and soluble in organic solvents (particularly common solvents capable of dissolving multiple polymers and curable compounds).
  • styrene-based resins from the viewpoints of transparency and weather resistance, styrene-based resins, (meth)acrylic resins, alicyclic olefin-based resins, polyester-based resins, cellulose derivatives (cellulose esters, etc.), etc. are preferred.
  • the hard coat layer 12 contains, for example, a binder resin and silica particles as a filler.
  • the silica particles preferably contain silica particles that have been surface-modified in advance.
  • Specific examples of the silane compound include vinyl group-containing silane compounds, (meth)acryloyl group-containing silane compounds, amino group-containing silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, epoxy group-containing silane compounds, and mercapto group-containing silane compounds. These may be used alone or in combination.
  • the silane compound is appropriately selected according to the type of binder resin, and when the binder resin contains a functional group, a silane compound having the same functional group as the binder resin is preferred.
  • the silane compound is preferably a (meth)acryloyl group-containing alkoxysilane compound.
  • (meth)acrylate refers to methacrylate and/or acrylate.
  • methacrylate and acrylate are treated as the same thing in terms of reaction mechanism.
  • the silane compound used for surface modification preferably has an alkoxysilyl group or a silanol group at its terminal, since this improves bonding with the hydroxyl groups present on the surface of the silica particles.
  • the dispersibility in the binder resin is improved, and the reaction between the surface treatment agent used for the surface modification and the binder resin causes the silica particles to bond more firmly to the binder resin, thereby improving the hardness of the optical laminate.
  • These silica particles may be exposed on the surface of the hard coat layer 12 on the optical functional layer 14 side. In this case, the hard coat layer 12 and the optical functional layer 14 are bonded more strongly via the adhesion layer 13. Examples of the method for exposing the silica particles include glow treatment described later, and in this case, the surface modification of the exposed silica surface is removed.
  • the filler is exposed on the surface of the hard coat layer, and the surface modification is removed at that time, so that an electrostatic attraction occurs between the hydroxyl groups generated on the filler surface and the adhesion layer 13 described below, and the adhesion is further improved.
  • the exposed filler also contributes to the improvement of adhesion by being embedded in the adhesion layer 13 as an anchor.
  • the improvement of flex resistance occurs due to a combination of the bonding with the binder resin by the surface modification of the silica surface described above and the interaction between the silica and the adhesion layer.
  • the average particle size of the filler in the hard coat layer 12 is, for example, 800 nm or less, preferably 780 nm or less, and more preferably 100 nm or less.
  • the haze value of the entire optical laminate 10 is 2% or less.
  • An optical laminate 10 with a haze of 2% or less has high transparency and serves as a so-called clear type anti-reflection film.
  • the surface of the hard coat layer 12 is preferably subjected to, for example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc.
  • glow discharge treatment is preferably used because it allows large-area treatment.
  • the strength of the glow discharge treatment can be, for example, 100 W/m 2 to 11,000 W/m 2 in terms of electrode power density, and is preferably 1,600 W/m 2 to 7,000 W/m 2 .
  • the average particle diameter of the filler of the hard coat layer 12 may be, for example, 0.5 ⁇ m or more.
  • a filler of this size for example, organic fine particles such as acrylic resin are preferably used.
  • the haze value of the entire optical laminate 10 is more than 2%.
  • the optical laminate 10 having a haze of more than 2% has anti-glare properties and becomes a so-called anti-glare (AG) type anti-reflection film.
  • the average particle diameter of the filler is preferably 10 ⁇ m or less, more preferably 5 ⁇ m or less, and particularly preferably 3 ⁇ m or less.
  • various reinforcing materials can be used within a range that does not impair the optical properties in order to impart toughness to the hard coat layer 12. Examples of the reinforcing materials include cellulose nanofibers.
  • the thickness of the hard coat layer 12 is not particularly limited, but is preferably 0.5 ⁇ m or more, and more preferably 1 ⁇ m or more.
  • the thickness of the hard coat layer 12 is preferably 100 ⁇ m or less.
  • the thickness of the hard coat layer 12 is 0.5 ⁇ m or more, sufficient hardness is obtained, making it difficult for scratches to occur during production.
  • the thickness of the hard coat layer 12 is 100 ⁇ m or less, the optical laminate 10 can be made thinner and lighter.
  • the thickness of the hard coat layer 12 is 100 ⁇ m or less, microcracks in the hard coat layer 12 that occur when the optical laminate 10 is bent during production are unlikely to occur, resulting in good productivity.
  • the hard coat layer 12 may be a single layer or a laminate of multiple layers.
  • the hard coat layer 12 may further be provided with known functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjusting function, and hardness adjusting function.
  • the function imparted to the hard coat layer 12 may be imparted to a single hard coat layer, or may be imparted to a plurality of separate layers.
  • the adhesion layer 13 is a layer formed to improve adhesion between the transparent substrate 11 or the hard coat layer 12, which is an organic film, and the optical function layer 14, which is an inorganic film.
  • the adhesion layer 13 is provided between the hard coat layer 12 and the optical function layer 14.
  • the adhesion layer 13 has a function of adhering the hard coat layer 12 and the optical function layer 14.
  • the adhesion layer 13 is preferably made of a metal oxide or metal in an oxygen-deficient state.
  • the metal oxide in an oxygen-deficient state refers to a metal oxide in a state in which the number of oxygen is deficient compared to the stoichiometric composition.
  • the metal oxide in an oxygen-deficient state examples include SiOx, AlOx, TiOx, ZrOx, CeOx, MgOx, ZnOx, TaOx, SbOx, SnOx, and MnOx.
  • the metal examples include Si, Al, Ti, Zr, Ce, Mg, Zn, Ta, Sb, Sn, Mn, and In.
  • the adhesion layer 13 may be, for example, SiOx, where x is more than 0 and less than 2.0.
  • the adhesion layer may be formed from a mixture of multiple types of metals or metal oxides.
  • the thickness of the adhesive layer is preferably more than 0 nm and not more than 20 nm, and particularly preferably 1 nm or more and not more than 10 nm.
  • the optical function layer 14 is a laminate that exhibits an anti-reflection function.
  • the optical function layer 14 shown in FIG. 2 is a laminate of a total of four layers, in which high refractive index layers 14a and low refractive index layers 14b are alternately laminated in this order from the adhesive layer 13 side.
  • the number of high refractive index layers 14a and low refractive index layers 14b is not particularly limited, and the number of high refractive index layers 14a and low refractive index layers 14b can be any number.
  • the optical function layer 14 is made of a laminate in which low refractive index layers 14b and high refractive index layers 14a are alternately laminated, so that the light incident from the anti-fouling layer 15 side interferes with each other through the optical function layer 14, thereby reducing the intensity of the reflected light and providing an anti-reflection function. Therefore, an anti-reflection function is obtained that prevents the light incident from the anti-fouling layer 15 side from being reflected in one direction.
  • the low refractive index layer 14b contains, for example, a metal oxide.
  • the low refractive index layer 14b may contain an oxide of Si from the viewpoints of availability and cost, and is preferably a layer mainly composed of SiO 2 (oxide of Si) or the like.
  • the SiO 2 single layer film is colorless and transparent.
  • the main component of the low refractive index layer 14b means a component contained in the low refractive index layer 14b at 50 mass % or more.
  • the low refractive index layer 14b is a layer mainly composed of an oxide of Si, it may contain less than 50 mass% of another element.
  • the content of the element other than the oxide of Si is preferably 10% or less.
  • the other element may contain Na for improving durability, Zr, Al, or N for improving hardness, and Zr and Al for improving alkali resistance.
  • the refractive index of the low refractive index layer 14b is preferably 1.20 to 1.60, and more preferably 1.30 to 1.50.
  • Examples of the dielectric material used for the low refractive index layer 14b include magnesium fluoride (MgF 2 , refractive index 1.38).
  • the refractive index of the high refractive index layer 14a is preferably 2.00 to 2.60, and more preferably 2.10 to 2.45.
  • dielectric materials used in the high refractive index layer 14a include niobium pentoxide (Nb 2 O 5 , refractive index 2.33), titanium oxide (TiO 2 , refractive index 2.33 to 2.55), tungsten oxide (WO 3 , refractive index 2.2), cerium oxide (CeO 2 , refractive index 2.2), tantalum pentoxide (Ta 2 O 5 , refractive index 2.16), zinc oxide (ZnO, refractive index 2.1), indium tin oxide (ITO, refractive index 2.06), and zirconium oxide (ZrO 2 , refractive index 2.2).
  • ITO or indium zinc oxide (IZO) can be selected.
  • the optical function layer 14 it is preferable to use, for example, a layer made of niobium pentoxide (Nb2O5, refractive index 2.33) as the high refractive index layer 14a and a layer made of SiO2 as the low refractive index layer 14b.
  • a layer made of niobium pentoxide Nb2O5, refractive index 2.33
  • a layer made of SiO2 SiO2
  • the thickness of the low refractive index layer 14b may be in the range of 1 nm to 200 nm, and is appropriately selected depending on the wavelength range in which the anti-reflection function is required.
  • the thickness of the high refractive index layer 14a may be, for example, from 1 nm to 200 nm, and is appropriately selected depending on the wavelength range in which the anti-reflection function is required.
  • the thicknesses of the high refractive index layer 14 a and the low refractive index layer 14 b can be appropriately selected depending on the design of the optical function layer 14 .
  • the layers may be a high refractive index layer 14a of 5 to 50 nm, a low refractive index layer 14b of 10 to 80 nm, a high refractive index layer 14a of 20 to 200 nm, and a low refractive index layer 14b of 50 to 200 nm.
  • a low refractive index layer 14b is disposed on the side of the antifouling layer 15. It is preferable that the low refractive index layer 14b of the optical functional layer 14 is in contact with the antifouling layer 15, since this improves the antireflection performance of the optical functional layer 14.
  • the antifouling layer 15 is formed on the outermost surface of the optical functional layer 14 and prevents the optical functional layer 14 from being soiled or damaged. Furthermore, when the antifouling layer 15 is applied to a touch panel or the like, it suppresses wear of the optical functional layer 14 due to its abrasion resistance.
  • the antifouling layer 15 of this embodiment is made of a vapor-deposited film formed by vapor-depositing an antifouling material.
  • the antifouling layer 15 is formed by vacuum-depositing a fluorine-based organic compound as the antifouling material on one surface of the low refractive index layer 14b constituting the optical function layer 14. In this embodiment, since the antifouling material contains a fluorine-based organic compound, the optical laminate 10 has even better abrasion resistance and alkali resistance.
  • the fluorine-based organic compound that constitutes the stain-resistant layer 15 is preferably a compound that comprises a fluorine-modified organic group and a reactive silyl group (e.g., alkoxysilane).
  • a fluorine-modified organic group e.g., alkoxysilane
  • Commercially available products include Optool DSX (manufactured by Daikin Corporation) and the KY-100 series (manufactured by Shin-Etsu Chemical Co., Ltd.).
  • the optical thickness of the anti-fouling layer 15 may be in the range of 1 nm or more and 20 nm or less, and is preferably in the range of 3 nm or more and 10 nm or less. If the thickness of the anti-fouling layer 15 is 1 nm or more, sufficient abrasion resistance can be ensured when the optical laminate 10 is applied to touch panel applications, etc. If the thickness of the anti-fouling layer 15 is 3 nm or more, the liquid resistance, etc. of the optical laminate 10 is improved. If the thickness of the anti-fouling layer 15 is 20 nm or less, the time required for vapor deposition is short, allowing for efficient production.
  • the ratio ((A)/(B)) of the Martens hardness (A) measured from the antifouling layer 15 side of the optical laminate 10, 102 to the Martens hardness measured from the hard coat layer 12 side of the laminate having only the transparent substrate 11 and the hard coat layer 12 is 3.6 or less (condition 1).
  • the above ratio ((A)/(B)) is preferably 3.5 or less, and more preferably 3.4 or less.
  • the optical laminate 10, 102 configured as described above, a friction tester using steel wool conforming to JIS L0849 is used, and the difference in contact angle with water before and after friction in which the steel wool is horizontally reciprocated 200 times is 20° or less (condition 2). If the optical laminate 10, 102 has a high hardness, the contact angle difference becomes 20° or less, and excellent scratch resistance can be achieved.
  • the elongation S (%) of the optical functional layer 14 calculated by the following formula (1) when a mandrel of the smallest diameter at which no cracks occur is used preferably satisfies 1.3 ⁇ S. This allows the bending resistance of the optical laminate 10, 102 to be further improved.
  • the compression ratio C (%) of the optical functional layer 14 calculated by the following formula (2) when a mandrel of the smallest diameter at which no cracks occur is used preferably satisfies 4.5 ⁇ C, and more preferably satisfies 5 ⁇ C. This allows the bending resistance of the optical laminate 10, 102 to be further improved.
  • the optical functional layer 14 satisfies both the above range of the elongation rate S (%) and the above range of the compression rate C (%). That is, in the optical laminate 10, 102, when the optical laminate 10, 102 is folded 180° so that the surface on which the antifouling layer 15 is formed is on the outside, the elongation rate S (%) of the optical functional layer 14 calculated by the following formula (1) satisfies 1.3 ⁇ S when a mandrel of the smallest diameter at which no cracks occur is used, and when the optical laminate 10, 102 is folded 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the compression rate C (%) of the optical functional layer 14 calculated by the above formula (2) satisfies 4.5 ⁇ C. This can further improve the bending resistance of the optical laminate 10, 102.
  • the above elongation rates are values when the substrate is PET and the thickness is 50 ⁇ m, and this value may vary if the thickness is reduced.
  • the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 4.0 ⁇ mm or less, more preferably 3.5 ⁇ mm or less, and even more preferably 3.0 ⁇ mm or less.
  • the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 1.1 ⁇ mm or less, and more preferably less than 1.0 ⁇ mm.
  • the thickness of the hard coat layer of the optical laminate is 5 ⁇ m
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 4.0 ⁇ mm or less
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 1.1 ⁇ mm or less.
  • the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 4.0 ⁇ mm or less, more preferably 3.5 ⁇ mm or less, and even more preferably 3.0 ⁇ mm or less.
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 1.4 ⁇ mm or less, and more preferably 1.2 ⁇ mm or less.
  • the thickness of the hard coat layer of the optical laminate is 10 ⁇ m
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 4.0 ⁇ mm or less
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 1.4 ⁇ mm or less.
  • the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 4.0 ⁇ mm or less, more preferably 3.5 ⁇ mm or less, and even more preferably 3.0 ⁇ mm or less.
  • the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel where the first crack was found is preferably 1.1 ⁇ mm or less, and more preferably less than 1.0 ⁇ mm.
  • the thickness of the hard coat layer of the optical laminate is 2 ⁇ m
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 4.0 ⁇ mm or less
  • the diameter of the mandrel is gradually changed to a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first found is 1.1 ⁇ mm or less.
  • the mandrel diameter mentioned above is calculated by cutting out three identical samples, measuring them, and averaging the three measurements.
  • the optical laminate 10 of this embodiment shown in FIG. 2 can be produced, for example, by the method described below.
  • a method for producing the optical laminate 10 a case in which the optical laminate 10 is produced using the transparent base material 11 wound in a roll shape will be described as an example.
  • the transparent substrate 11 wound in a roll shape is unwound.
  • a slurry containing a material to be the hard coat layer 12 is applied onto the transparent substrate 11 by a known method, and cured by a known method corresponding to the material to be the hard coat layer 12.
  • the slurry used may be, for example, a composition containing a binder resin and silica particles as a filler, and this composition is applied onto the transparent substrate 11 and then cured. This forms the hard coat layer 12 on the transparent substrate 11 (hard coat layer forming process).
  • the composition may contain one or more additives such as a polymerization initiator and a leveling agent as necessary.
  • a polymerization initiator for example, a photopolymerization initiator is used.
  • the transparent substrate 11 on which the hard coat layer 12 is formed is wound into a roll shape by a known method.
  • an adhesion layer forming process is performed to form an adhesion layer 13 on the hard coat layer 12, and an optical function layer forming process is performed to form an optical function layer 14.
  • an anti-fouling layer forming process is performed to form an anti-fouling layer 15 on the optical function layer 14.
  • a second surface treatment process to treat the surface of the optical function layer 14 after the optical function layer forming process, and then perform the anti-fouling layer forming process.
  • the first surface treatment step, the adhesion layer forming step, the optical functional layer forming step, the second surface treatment step, and the antifouling layer forming step are performed successively while the optical laminate in the middle of manufacture is maintained under reduced pressure.
  • a sputtering device equipped with the thin film forming device described in Patent Document 4 can be used.
  • a specific example of a manufacturing apparatus that can be used in the method for manufacturing the optical laminate of this embodiment is a manufacturing apparatus 20 shown in FIG.
  • the manufacturing apparatus 20 shown in Fig. 3 includes a roll unwinding device 4, a pretreatment device 2A, a sputtering device 1, a pretreatment device 2B, a vapor deposition device 3, and a roll winding device 5. As shown in Fig. 3, these devices 4, 2A, 1, 2B, 3, and 5 are connected in this order.
  • the manufacturing apparatus 20 shown in Fig. 3 is a roll-to-roll type manufacturing apparatus that unwinds a substrate from a roll, passes the substrate through connected devices (pretreatment device 2A, sputtering device 1, pretreatment device 2B, and vapor deposition device 3 in Fig. 3) in succession, and then winds the substrate, thereby continuously forming multiple layers on the substrate.
  • the conveying speed (line speed) of the optical laminate 10 during manufacture can be set appropriately.
  • the conveying speed is preferably, for example, 0.5 to 20 m/min, and more preferably 0.5 to 10 m/min.
  • the roll unwinding device 4 shown in Fig. 3 has a chamber 34 inside which a predetermined reduced pressure atmosphere is maintained, one or more vacuum pumps 21 (one in Fig. 3) that exhaust gas from within the chamber 34 to create a reduced pressure atmosphere, and an unwinding roll 23 and a guide roll 22 installed within the chamber 34.
  • the chamber 34 is connected to the chamber 31 of the sputtering device 1 via a pretreatment device 2A.
  • the transparent substrate 11 having the hard coat layer 12 formed on the surface thereof is wound around the unwinding roll 23.
  • the unwinding roll 23 supplies the transparent substrate 11 having the hard coat layer 12 formed on the surface thereof to the pretreatment device 2A at a predetermined transport speed.
  • the pretreatment device 2A shown in Fig. 3 has a chamber 32 with a predetermined reduced pressure atmosphere inside, a can roll 26, a plurality of (two in Fig. 3) guide rolls 22, and a plasma discharge device 42. As shown in Fig. 3, the can roll 26, the guide roll 22, and the plasma discharge device 42 are installed in the chamber 32. As shown in Fig. 3, the chamber 32 is connected to the chamber 31 of the sputtering device 1.
  • the can roll 26 and the guide roll 22 transport the transparent substrate 11 on which the hard coat layer 12 has been formed, which has been sent from the roll unwinding device 4, at a predetermined transport speed, and send the transparent substrate 11 on which the surface of the hard coat layer 12 has been treated, to the sputtering device 1.
  • the plasma discharge device 42 is disposed facing the outer peripheral surface of the can roll 26 at a predetermined distance.
  • the plasma discharge device 42 ionizes the gas by glow discharge.
  • the gas is preferably inexpensive, inert, and does not affect the optical characteristics, and examples of the gas that can be used include argon gas, oxygen gas, nitrogen gas, and helium gas. In this embodiment, it is preferable to use argon gas or oxygen gas as the gas.
  • the sputtering apparatus 1 shown in Fig. 3 includes a chamber 31 with a predetermined reduced pressure atmosphere inside, one or more vacuum pumps 21 (two in Fig. 3) that exhaust gas from the chamber 31 to create a reduced pressure atmosphere, a film-forming roll 25, a plurality of guide rolls 22 (two in Fig. 4), and a plurality of film-forming units 41 (four in the example shown in Fig. 3).
  • the film-forming roll 25, the guide roll 22, and the film-forming units 41 are installed in the chamber 31.
  • the chamber 31 is connected to a chamber 32 of a pretreatment device 2B.
  • the film-forming roll 25 and the guide roll 22 transport the transparent substrate 11 having the surface-treated hard coat layer 12 formed thereon, which has been sent from the pre-processing device 2A, at a predetermined transport speed, and supply the transparent substrate 11 having the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12 to the pre-processing device 2B.
  • an adhesion layer 13 is laminated by sputtering on the hard coat layer 12 of the transparent substrate 11 running on a film-forming roll 25, and high refractive index layers 14a and low refractive index layers 14b are alternately laminated on top of the adhesion layer 13 to form an optically functional layer 14.
  • the film forming unit 41 is disposed facing the outer peripheral surface of the film forming roll 25 at a predetermined interval, and a plurality of film forming units 41 are provided to surround the film forming roll 25.
  • the number of film forming units 41 is determined according to the total number of layers of the adhesive layer 13 and the high refractive index layer 14a and the low refractive index layer 14b forming the optical functional layer 14.
  • a plurality of film forming rolls 25 may be provided in the chamber 31, and the film forming unit 41 may be disposed around each film forming roll 25.
  • a guide roll 22 may be further provided as necessary.
  • a plurality of chambers 31 provided with the film forming rolls 25 and the film forming units 41 may be connected.
  • the diameter of the film forming roll 25 may be appropriately changed to make it easier to ensure the distance between adjacent film forming units 41.
  • Each deposition section 41 is provided with a specific target (not shown). A voltage is applied to the target using a known structure.
  • a gas supply section (not shown) that supplies a specific reactive gas and carrier gas to the target at a specific flow rate, and a known magnetic field generating source (not shown) that forms a magnetic field on the surface of the target are provided near the target.
  • the target material and the type and flow rate of the reactive gas are appropriately determined according to the composition of the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b formed on the transparent substrate 11 by passing between the film forming unit 41 and the film forming roll 25.
  • SiO 2 Si is used as the target and O 2 is used as the reactive gas.
  • Nb is used as the target and O 2 is used as the reactive gas.
  • the low refractive index layer 14b is preferably formed at a vacuum degree of less than 0.5 Pa
  • the high refractive index layer 14a is preferably formed at a vacuum degree of less than 1.0 Pa.
  • magnetron sputtering As the sputtering method, from the viewpoint of increasing the film formation speed, it is preferable to use magnetron sputtering as the sputtering method.
  • the sputtering method is not limited to magnetron sputtering, and a two-pole sputtering method using plasma generated by direct current glow discharge or high frequency, or a three-pole sputtering method with an additional hot cathode may also be used.
  • the sputtering apparatus 1 is equipped with an optical monitor (not shown) as a measuring unit that measures optical characteristics after the layers that become the adhesion layer 13 and the optical functional layer 14 are formed. This makes it possible to check the quality of the adhesion layer 13 and the optical functional layer 14 that are formed. If the sputtering apparatus 1 has, for example, two or more chambers, it is preferable to install an optical monitor in each chamber.
  • An example of an optical monitor is one that uses an optical head capable of scanning in the width direction to measure the optical characteristics in the width direction of the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12.
  • an optical monitor for example, the peak wavelength of reflectance can be measured as the optical characteristic, and the optical thickness distribution in the width direction of the adhesion layer 13 and the optical functional layer 14 can be measured by converting it into optical thickness.
  • the pretreatment device 2B shown in Fig. 3 has a chamber 32 with a predetermined reduced pressure atmosphere inside, a can roll 26, a plurality of (two in Fig. 3) guide rolls 22, and a plasma discharge device 42. As shown in Fig. 3, the can roll 26, the guide roll 22, and the plasma discharge device 42 are installed in the chamber 32. As shown in Fig. 3, the chamber 32 is connected to a chamber 33 of the deposition device 3.
  • the can roll 26 and the guide roll 22 transport the transparent substrate 11, on which each layer up to the optical functional layer 14 has been formed, sent from the sputtering device 1 at a predetermined transport speed, and send the transparent substrate 11, on which the surface of the optical functional layer 14 has been treated, to the deposition device 3.
  • the plasma discharge device 42 for example, one similar to the pretreatment device 2A can be used.
  • the deposition apparatus 3 shown in Fig. 4 includes a chamber 33 having a predetermined reduced pressure atmosphere inside, one or more vacuum pumps 21 (one in Fig. 3) that exhaust gas from the chamber 33 to create a reduced pressure atmosphere, a plurality of guide rolls 22 (four in Fig. 3), a deposition source 43, and a heating device 53. As shown in Fig. 3, the guide rolls 22 and the deposition source 43 are installed in the chamber 33.
  • the chamber 33 is connected to a chamber 35 of the roll winding device 5.
  • the vapor deposition source 43 is disposed opposite to the transparent substrate 11 having the treated surface of the optical functional layer 14, which is transported substantially horizontally between two adjacent guide rolls 22.
  • the vapor deposition source 43 supplies an evaporated gas made of a material that will become the antifouling layer 15 onto the optical functional layer 14.
  • the orientation of the vapor deposition source 43 can be set arbitrarily.
  • the heating device 53 heats the material that will become the antifouling layer 15 to the vapor pressure temperature.
  • the heating device 53 may be one that uses a resistance heating method, a heater heating method, an induction heating method, an electron beam method, or the like.
  • a container that contains the antifouling material that will become the antifouling layer 15 is used as a resistor and electrically heated.
  • the container is heated by a heater disposed on the outer periphery of the container.
  • the induction heating method the container or the antifouling material is heated by electromagnetic induction from an induction coil installed externally.
  • the vapor deposition apparatus 3 shown in FIG. 3 includes a guide plate (not shown) for guiding the vapor deposition material evaporated by the vapor deposition source 43 to a predetermined position, a film thickness gauge (not shown) for observing the thickness of the antifouling layer 15 formed by vapor deposition, a vacuum pressure gauge (not shown) for measuring the pressure inside the chamber 33, and a power supply (not shown).
  • the guide plate may have any shape as long as it can guide the evaporated deposition material to a desired position. If the guide plate is not necessary, it does not have to be provided.
  • the vacuum pressure gauge for example, an ion gauge can be used.
  • the power supply device may be, for example, a high frequency power supply.
  • the roll winding device 5 shown in Figure 3 has a chamber 35 inside which a predetermined reduced pressure atmosphere is maintained, one or more vacuum pumps 21 (one in Figure 3) that exhaust gas from within the chamber 35 to create a reduced pressure atmosphere, and a winding roll 24 and a guide roll 22 installed within the chamber 35.
  • the transparent substrate 11 optical laminate 10) on whose surface each layer up to the antifouling layer 15 is formed is wound around the winding roll 24.
  • the winding roll 24 and the guide roll 22 wind up the optical laminate 10 at a predetermined winding speed. If necessary, a carrier film may also be used.
  • the vacuum pump 21 provided in the manufacturing apparatus 20 shown in FIG. 4 may be, for example, a dry pump, an oil rotary pump, a turbo molecular pump, an oil diffusion pump, a cryopump, a sputter ion pump, or a getter pump.
  • the vacuum pumps 21 may be appropriately selected or combined to create the desired reduced pressure state in each of the chambers 31, 32, 33, 34, and 35.
  • the vacuum pump 21 may be installed at any position and in any number in the manufacturing apparatus 20 as long as it can maintain both the chamber 31 of the sputtering apparatus 1 and the chamber 33 of the deposition apparatus 3 at the desired reduced pressure.
  • the vacuum pump 21 may be installed in each of the chambers 31, 32, 33, 34, and 35, or may be installed in only some of the chambers 31, 32, 33, 34, and 35 as long as it can maintain both the chamber 31 of the sputtering apparatus 1 and the chamber 33 of the deposition apparatus 3 at the desired reduced pressure.
  • the unwinding roll 23 around which the transparent substrate 11 having the hard coat layer 12 formed on its surface is wound is placed in the chamber 34 of the roll unwinding device 4. Then, the unwinding roll 23 and the guide roll 22 are rotated to send the transparent substrate 11 having the hard coat layer 12 formed on its surface to the pretreatment device 2A at a predetermined transport speed.
  • a first surface treatment step is performed as a pretreatment for the surface on which the adhesion layer 13 and the optical functional layer 14 are to be formed.
  • the first surface treatment step is performed on the transparent substrate 11 on which the hard coat layer 12 is formed.
  • the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11 on which the hard coat layer 12 is formed at a predetermined transport speed, while treating the surface of the hard coat layer 12 running on the can roll 26.
  • the surface treatment method of the hard coat layer 12 can be, for example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc. As mentioned above, among these, it is preferable to use glow discharge treatment because it allows for large area treatment.
  • the adhesion layer forming process and the optical function layer forming process are performed in the chamber 31 of the sputtering device 1. Specifically, the film-forming roll 25 and the guide roll 22 are rotated to transport the transparent substrate 11 on which the hard coat layer 12 has been formed at a predetermined transport speed, while the adhesion layer 13 and the optical function layer 14 are formed on the hard coat layer 12 running on the film-forming roll 25.
  • the adhesive layer 13 is formed by sputtering while changing the material of the target placed in each film forming section 41 or the type and flow rate of the reactive gas supplied from the gas supply section, and the high refractive index layer 14a and the low refractive index layer 14b are alternately laminated thereon. That is, the adhesive layer forming process and the optical function layer forming process are performed continuously in the sputtering apparatus 1. In this way, the adhesive layer 13 and the optical function layer 14, which is an anti-reflection layer, are formed.
  • the high refractive index layer 14a and the low refractive index layer 14b are formed under conditions of a predetermined vacuum degree or less. Specifically, the high refractive index layer 14a is formed at a vacuum degree of less than 1.0 Pa, and the low refractive index layer 14b is formed at a vacuum degree of less than 0.5 Pa.
  • the adhesion layer 13 When a SiOx film is formed as the adhesion layer 13, it is preferable to form the adhesion layer 13 by reactive sputtering using a silicon target in a mixed gas atmosphere of oxygen gas and argon gas.
  • the target material may be changed when forming the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b.
  • one type of material may be used as a target, and a flow rate of oxygen (reactive gas) during sputtering may be changed to alternately form layers made of the target material and layers made of an oxide of the target material, forming the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b.
  • a flow rate of oxygen (reactive gas) during sputtering may be changed to alternately form layers made of the target material and layers made of an oxide of the target material, forming the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b.
  • the pressure during sputtering to form the adhesion layer 13 and the optical function layer 14 varies depending on the metal being sputtered, but may be 2 Pa or less, preferably 1 Pa or less, more preferably 0.6 Pa or less, and particularly preferably 0.2 Pa or less.
  • the pressure during sputtering is reduced to 1 Pa or less, the mean free path of the film-forming molecules becomes longer and the film-forming molecules are laminated while maintaining their high energy, resulting in a denser and better film quality.
  • the pressure during sputtering of the high refractive index layer and the low refractive index layer be different. This is because the mean free path differs for each type of film. By changing the pressure for each type of film, a denser film can be formed.
  • the transparent substrate 11 having the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12 is sent to the pretreatment device 2B by the rotation of the film-forming roll 25 and the guide roll 22 .
  • a second surface treatment step is performed as a pretreatment for the surface on which the antifouling layer 15 is to be formed.
  • the transparent substrate 11 on which the optical functional layer 14 has been formed, obtained by the optical functional layer forming step, is continuously subjected to the second surface treatment step while being maintained under reduced pressure without being exposed to the air.
  • the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11, on which each layer up to the optical functional layer 14 has been formed, at a predetermined transport speed, while a discharge treatment is performed on the surface of the optical functional layer 14 running on the can roll 26.
  • the surface treatment method for the optical functional layer 14 can be, for example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc. Among these, it is preferable to use glow discharge treatment because it allows for large area treatment.
  • the surface condition of the optical functional layer 14 is expressed by the surface roughness Ra or the average length of the elements RSm.
  • the surface condition of the optical functional layer 14 is easily defined by the surface roughness Ra.
  • the surface condition of the optical functional layer 14 is easily defined by the average length of the elements RSm.
  • the surface roughness Ra and the average length of the elements RSm are measured in accordance with JIS B0601 (ISO4287).
  • the transparent substrate 11 with the surface of the optical functional layer 14 treated is sent to the deposition device 3 by the rotation of the can roll 26 and the guide roll 22 .
  • an antifouling layer forming step is performed in the chamber 33 of the deposition device 3.
  • the transparent substrate 11 having the treated surface of the optical functional layer 14 obtained by the second surface treatment step is continuously subjected to the antifouling layer forming step while being maintained under reduced pressure without being exposed to the air.
  • the guide roll 22 is rotated to transport the transparent substrate 11 having the treated surface of the optical functional layer 14 at a predetermined transport speed, while the deposition source 43 is deposited on the surface of the optical functional layer 14 .
  • an antifouling material made of a fluorine-based organic compound that becomes the antifouling layer 15 is heated to a vapor pressure temperature by a heating device 53, and the resulting evaporated gas is supplied from a deposition source 43 in a reduced pressure environment and adhered to the optical function layer 14 whose surface has been treated, thereby forming the antifouling layer 15 by vacuum deposition.
  • the pressure during vacuum deposition of the antifouling layer 15 is, for example, preferably 0.05 Pa or less, more preferably 0.01 Pa or less, and particularly preferably 0.001 Pa or less.
  • the above method provides an optical laminate 10 in which an antifouling layer 15 is formed by vacuum deposition on an adhesion layer 13 and an optical functional layer 14 formed by sputtering. After deposition, the antifouling layer 15 preferably has an initial fluorine content of 0.03 or more as measured using X-ray fluorescence analysis (XRF).
  • XRF X-ray fluorescence analysis
  • the transparent substrate 11 (optical laminate 10 ) on which each layer up to the antifouling layer 15 has been formed is sent to the roll winding device 5 by the rotation of the guide roll 22 .
  • the optical laminate 10 is wound around the winding roll 24 by the rotation of the winding roll 24 and the guide roll 22 .
  • the optical functional layer forming process and the antifouling layer forming process are preferable to perform the optical functional layer forming process and the antifouling layer forming process continuously under reduced pressure.
  • the optical laminate 10 is continuously manufactured as a wound body by a roll-to-roll method, as in the manufacturing method of this embodiment using the manufacturing apparatus 20 shown in FIG. 3, it is more preferable to perform the optical functional layer forming process and the antifouling layer forming process continuously in-line while maintaining a reduced pressure state.
  • In-line means that the antifouling layer forming process is performed without exposing the optical functional layer 14 formed in the optical functional layer forming process to the air.
  • the optical functional layer forming process and the antifouling layer forming process By performing the optical functional layer forming process and the antifouling layer forming process continuously under reduced pressure, the generation of a natural oxide film on the optical functional layer 14 formed in the optical functional layer forming process before the antifouling layer 15 is formed is suppressed. In addition, contamination such as foreign matter when winding the roll can be prevented from adhering to the optical functional layer 14 and inhibiting the adhesion between the optical functional layer 14 and the antifouling layer 15.
  • the anti-fouling layer 15 of the optical laminate 10 of this embodiment is a vapor deposition film, it has high abrasion resistance compared to, for example, an anti-fouling film formed by a coating method. This is presumably due to the following reasons. In other words, in an anti-fouling film formed by a coating method, there are voids due to the solvent contained in the paint. In contrast, there are no voids due to the solvent in a vapor deposition film. For this reason, it is presumed that a vapor deposition film has a high density and has high abrasion resistance and alkali resistance compared to an anti-fouling film formed by a coating method.
  • the manufacturing method for the optical laminate 10 of this embodiment includes an adhesion layer forming step of forming an adhesion layer 13, an optical function layer forming step of forming an optical function layer 14 by alternately laminating high refractive index layers 14a and low refractive index layers 14b, a second surface treatment step of treating the surface of the optical function layer 14, and an anti-stain layer forming step of forming an anti-stain layer 15 on the surface-treated optical function layer 14.
  • an adhesion between the optical function layer 14 and the anti-stain layer 15 formed on the optical function layer 14 is good, and the abrasion resistance and alkali resistance are further improved.
  • the reduced pressure conditions in the chambers of, for example, the sputtering device and the deposition device may be different as long as they do not interfere with each production process.
  • the film formation results it is preferable to measure the film formation results over time using a measuring device in one or more of the adhesion layer formation process, optical function layer formation process, and antifouling layer formation process, and feed back the results to the conditions of the subsequent manufacturing process.
  • a measuring device in one or more of the adhesion layer formation process, optical function layer formation process, and antifouling layer formation process, and feed back the results to the conditions of the subsequent manufacturing process.
  • the measuring device can also be used to provide feedback on the manufacturing conditions in the same process. In this case, the layer formed in that process will have uniform and stable characteristics.
  • the second surface treatment step is performed between the optical functional layer forming step and the antifouling layer forming step, but the second surface treatment step may be performed as necessary, and does not have to be performed. Even in cases in which the second surface treatment step is not performed, it is preferable to perform the optical functional layer forming step and the antifouling layer forming step consecutively under reduced pressure.
  • the optical functional layer is formed under conditions of a predetermined vacuum level or less.
  • the optical functional layer 14 becomes dense, the water vapor permeability decreases, and the abrasion resistance and alkali resistance improve.
  • the antifouling layer have a thickness of a predetermined thickness or more, sufficient scratch resistance and alkali resistance can be ensured.
  • the manufacturing apparatus 20 shown in FIG. 3 which is equipped with a pre-processing device 2A, a sputtering device 1, a pre-processing device 2B, a vapor deposition device 3, a roll unwinding device 4, and a roll winding device 5.
  • the manufacturing apparatus for manufacturing the optical laminate 10 is not limited to the manufacturing apparatus 20 shown in FIG. 3.
  • a manufacturing apparatus may be used that does not include pretreatment devices 2A and 2B, and that has roll unwinding device 4, sputtering device 1, deposition device 3, and roll winding device 5 connected in this order.
  • the manufacturing apparatus 20 shown in FIG. 3 may be provided with a pretreatment chamber (not shown) between the chamber 33 of the vapor deposition apparatus 3 and the chamber 32 of the pretreatment apparatus 2B for cleaning the surface of the optical functional layer 14 on which the antifouling layer 15 is to be formed.
  • the manufacturing apparatus 20 shown in FIG. 3 may be provided with a post-treatment chamber (not shown) between the chamber 33 of the vapor deposition apparatus 3 and the chamber 35 of the roll winding apparatus 5 for cooling and/or inspecting the transparent substrate 11 on which each layer up to the antifouling layer 15 has been formed.
  • the manufacturing apparatus 20 shown in FIG. 3 may be provided with a hard coat layer forming device between the roll unwinding device 4 and the sputtering device 1 for forming a hard coat layer 12 on the surface of the transparent substrate 11.
  • a hard coat layer forming device between the roll unwinding device 4 and the sputtering device 1 for forming a hard coat layer 12 on the surface of the transparent substrate 11.
  • the optical functional layer 14 and the antifouling layer 15 but also the hard coat layer 12 can be manufactured continuously by the roll-to-roll method, which is preferable.
  • optical functional layer formation process is performed using a sputtering device and the antifouling layer formation process is performed using a deposition device, but if the second surface treatment process is not performed, the optical functional layer formation process and the antifouling layer formation process may be performed in the same device (within one chamber).
  • various layers may be provided as necessary on the surface of the transparent substrate opposite the surface on which the optical functional layer and the like are formed.
  • an adhesive layer used for adhesion to other members may be provided.
  • other optical films may be provided via this adhesive layer. Examples of other optical films include polarizing films, phase difference compensation films, films that function as half-wave plates, and quarter-wave plates.
  • a layer having functions such as antireflection, selective reflection, antiglare, polarization, phase difference compensation, viewing angle compensation or expansion, light guiding, diffusion, brightness improvement, hue adjustment, and electrical conductivity may be formed directly on the opposing surface of the transparent substrate.
  • the optical laminate may have a smooth shape, or may have a nano-order uneven structure that exhibits a moth-eye or anti-glare function. It may also have a geometric shape of micro to millimeter order such as a lens or prism.
  • the shape can be formed by, for example, a combination of photolithography and etching, shape transfer, heat pressing, or the like. In this embodiment, since the film is formed by deposition or the like, even if the substrate has an uneven shape, the uneven shape can be maintained.
  • the article of this embodiment is, for example, a liquid crystal display panel, an organic EL display panel, or the like, in which the above-mentioned optical laminate 10 is provided on the display surface of an image display unit.
  • This makes it possible to impart high abrasion resistance and alkali resistance to, for example, the touch panel display unit of a smartphone or an operating device, and to realize an image display device that is highly durable and suitable for practical use.
  • the article is not limited to image display devices, but may be any article to which the optical laminate 10 can be applied, such as window glass or goggles with the optical laminate of this embodiment on the surface, the light receiving surface of a solar cell, the screen of a smartphone or a display such as a notebook PC, information input terminals, tablet terminals, AR (augmented reality) devices, VR (virtual reality) devices, electronic display boards, glass table surfaces, gaming machines, navigation support devices such as aircraft and trains, navigation systems, instrument panels, and the surface of optical sensors.
  • the optical laminate 10 such as window glass or goggles with the optical laminate of this embodiment on the surface, the light receiving surface of a solar cell, the screen of a smartphone or a display such as a notebook PC, information input terminals, tablet terminals, AR (augmented reality) devices, VR (virtual reality) devices, electronic display boards, glass table surfaces, gaming machines, navigation support devices such as aircraft and trains, navigation systems, instrument panels, and the surface of optical sensors.
  • optical laminates produced in the following examples and comparative examples are examples that function as anti-reflection films, and the scope of the present invention is not limited to these.
  • composition 1 was prepared, in which the content of silica particles (filler) having an average particle size of 50 nm was 28 mass % relative to the total solid content of the composition. As shown in Table 1, composition 1 was prepared by dissolving acrylate (binder resin), silica particles, and a photopolymerization initiator in a solvent, and further adding a leveling agent.
  • CN968 6-functional aliphatic urethane acrylate having a polyester skeleton
  • SR610 Polyethylene glycol diacrylate, average molecular weight of polyethylene glycol chain: 600
  • PGM-AC-4130Y Surface-modified silica sol with methacryloyl group-containing silane compound, dispersion medium: propylene glycol monomethyl ether
  • Ominirad 184 1-hydroxy-cyclohexyl-phenyl-ketone
  • Example 1 A 50 ⁇ m-thick PET film was used as a transparent substrate, and the above composition 1 was applied onto this PET film with a bar coater, and then the composition 1 was photopolymerized to form a 5 ⁇ m-thick hard coat layer on the transparent substrate.
  • the surface of the hard coat layer was subjected to a surface treatment by glow discharge treatment with an electrode power density of 5500 W/m 2.
  • an adhesive layer and an optical functional layer were successively formed on the hard coat layer by a reactive sputtering method using a Si target and a Nb target as sputtering targets and a mixed gas of Ar gas and O 2 gas.
  • SiOx silicon oxide
  • a 3 nm thick antifouling layer made of an alkoxysilane compound having a perfluoropolyether group (KY1903-1, manufactured by Shin-Etsu Chemical Co., Ltd.) was formed by deposition on the SiO 2 film of the topmost layer of the optical functional layer at a pressure of 0.01 Pa in the deposition chamber, a deposition temperature of 230° C., and a retention time of 7.2 s to produce an optical laminate (antireflection film) of the example.
  • Example 2 An optical laminate was obtained in the same manner as in Example 1, except that the electrode power density during the glow discharge treatment was changed from 5500 W/ m2 to 1100 W/ m2 .
  • Example 3 An optical laminate was obtained in the same manner as in Example 1, except that the electrode power density in the glow discharge treatment was changed from 5500 W/ m2 to 6600 W/ m2 .
  • Example 4 An optical laminate was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 2 ⁇ m.
  • Example 5 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 2.
  • Example 6 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 3.
  • Example 7 An optical laminate was obtained in the same manner as in Example 1, except that a 23 ⁇ m thick PET film was used as the transparent substrate instead of the 50 ⁇ m thick PET film.
  • Example 8 An optical laminate was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 10 ⁇ m.
  • Example 9 An optical laminate was obtained in the same manner as in Example 8, except that the electrode power density during the glow discharge treatment was changed from 5500 W/ m2 to 3300 W/ m2 .
  • Example 10 An optical laminate was obtained in the same manner as in Example 8, except that the electrode power density during the glow discharge treatment was changed from 5500 W/ m2 to 1100 W/ m2 .
  • Example 11 An optical laminate was obtained in the same manner as in Example 8, except that the electrode power density during the glow discharge treatment was changed from 5500 W/ m2 to 550 W/ m2 .
  • composition 1 forming the hard coat layer was changed to the composition 4 shown in Table 1, and the electrode power density during the glow discharge treatment was set to 5000 W / m 2.
  • An optical laminate was obtained in the same manner as in Example 1.
  • Comparative Example 2 An optical laminate was obtained in the same manner as in Comparative Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 10 ⁇ m and the electrode power density during the glow discharge treatment was changed from 5000 W / m 2 to 1100 W / m 2 .
  • optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated using the following methods.
  • ⁇ Bending test> As a sample, an optical laminate was cut into a size of 1 cm x 15 cm to prepare a sample. It was confirmed that the optical laminate had no cracks on the cut surface.
  • a 5.0 mm mandrel was set in a bending tester capable of setting a mandrel. The optical laminate described above was set in this tester so that the surface on which the antifouling layer was formed was bent outward. The tester was then bent over 2 seconds to bend the optical laminate 180° and held for 10 seconds. Thereafter, the presence or absence of cracks in the antifouling layer was confirmed visually and by an optical microscope.
  • the above procedure was repeated, changing the mandrel diameter to a smaller one every 0.2 mm, until abnormalities such as cracks were found on the surface of the antifouling layer side of the optical laminate by visual inspection and optical microscope, and the diameter ( ⁇ mm) of the mandrel that was 0.2 mm larger than the diameter of the mandrel where the first crack was found was recorded as the test result of the bending test.
  • measurements were also taken when the optical laminate was set in the above-mentioned testing machine so that the surface on which the antifouling layer was formed was folded inward, and the mandrel diameter ( ⁇ mm) that was 0.2 mm larger than the mandrel diameter at which the first crack was discovered was taken as the test result of the bending test.
  • the theoretical elongation percentage S (%) of the optical functional layer was calculated when a mandrel with the smallest diameter at which no cracks were generated was used.
  • ⁇ Martens hardness> Using each of the compositions 1 to 4, a laminate (sample) in which only a hard coat layer was formed on a transparent substrate was prepared. For the optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2, the Martens hardness of the antifouling layer side of the optical laminate was measured. For the laminates in which only a hard coat layer was formed, the Martens hardness of the hard coat layer side of the laminate was measured. For the measurement, a microcompression tester (ENT-NEXUS, manufactured by Elionix, measuring indenter: Berkovich indenter) was used in accordance with ISO14577-1.
  • ENT-NEXUS manufactured by Elionix, measuring indenter: Berkovich indenter
  • the hardness was measured at an indentation depth of 50 nm, and for the laminates in which only a hard coat layer was formed, the hardness was measured when indented to a depth of 1/10 of the thickness of the hard coat layer.
  • the Martens hardness of the optical laminate measured above was taken as (A)
  • the Martens hardness of the laminate in which only the hard coat layer was formed on the transparent substrate was taken as (B)
  • the ratio (A)/(B) was calculated. The results are shown in Table 2.
  • optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.
  • DM-700 manufactured by Kyowa Interface Science Co., Ltd.
  • the silica particles contained in the hard coat layer are surface-modified with methacryloyl groups derived from a methacryloyl group-containing silane compound, and therefore the methacryloyl groups are more firmly bonded to the acrylate (binder resin), and as a result, the hardness of the optical laminate is improved. Furthermore, it was found that the methacryloyl groups on the silica particle surface further improve the adhesion between the hard coat layer and the adhesive layer, and between the optical functional layer via the adhesive layer, and the bending resistance is further improved. Furthermore, in all of Examples 1 to 7, the difference in contact angle with water before and after rubbing, in which the steel wool was moved back and forth horizontally 200 times, was 20° or less.
  • the silica particles contained in the hard coat layer are surface-modified with methacryloyl groups derived from the methacryloyl group-containing silane compound, and the methacryloyl groups are more firmly bonded to the acrylate (binder resin).
  • the hardness of the optical laminate was improved and excellent scratch resistance could be achieved.
  • Comparative Example 1 when a hard coat layer was formed using Composition 4 containing silica particles that had not been surface-modified, the ratio ((A)/(B)) was 3.71, and the hardness of the laminate was low. In addition, the elongation rate S (outer bending) was 1.22, and the compression rate C (inner bending) was 4.4, and the flex resistance was poor.
  • Comparative Example 2 when a hard coat layer was formed using Composition 2 containing silica particles that had not been surface-modified, the contact angle difference was 23.6°, and a decrease in scratch resistance was observed. In addition, the elongation rate S (outward bending) was 1.29, and the compression rate C (inward bending) was 3.63, and bending resistance was poor.
  • Reference Signs List 10 102: Optical laminate 11: Transparent substrate 12: Hard coat layer 13: Adhesion layer 14: Optical functional layer 14a: High refractive index layer 14b: Low refractive index layer 15: Antifouling layer 20: Manufacturing apparatus 1: Sputtering apparatus 2A, 2B: Pretreatment apparatus 3: Vapor deposition apparatus 4: Roll unwinding apparatus 5: Roll winding apparatus 20: Manufacturing apparatus 21: Vacuum pump 22: Guide roll 23: Unwinding roll 24: Winding roll 25: Film-forming roll 26: Can roll 31, 32, 33, 34, 35: Chamber 41: Film-forming section 42: Plasma discharge apparatus 43: Vapor deposition source 53: Heating apparatus

Landscapes

  • Physics & Mathematics (AREA)
  • General Physics & Mathematics (AREA)
  • Optics & Photonics (AREA)
  • Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Inorganic Chemistry (AREA)
  • Laminated Bodies (AREA)
  • Surface Treatment Of Optical Elements (AREA)
PCT/JP2024/016571 2023-04-28 2024-04-26 光学積層体及びこれを備えた物品 Ceased WO2024225472A1 (ja)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN202480026779.6A CN121002404A (zh) 2023-04-28 2024-04-26 光学层叠体及具备该光学层叠体的物品
KR1020257034507A KR20250168355A (ko) 2023-04-28 2024-04-26 광학 적층체 및 이것을 구비한 물품

Applications Claiming Priority (6)

Application Number Priority Date Filing Date Title
JP2023-074698 2023-04-28
JP2023074698 2023-04-28
JP2024063462 2024-04-10
JP2024-063462 2024-04-10
JP2024069031A JP7850197B2 (ja) 2023-04-28 2024-04-22 光学積層体、これを備えた物品及び光学積層体の製造方法
JP2024-069031 2024-04-22

Publications (1)

Publication Number Publication Date
WO2024225472A1 true WO2024225472A1 (ja) 2024-10-31

Family

ID=93256879

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/016571 Ceased WO2024225472A1 (ja) 2023-04-28 2024-04-26 光学積層体及びこれを備えた物品

Country Status (4)

Country Link
JP (2) JP7850197B2 (enExample)
KR (1) KR20250168355A (enExample)
CN (1) CN121002404A (enExample)
WO (1) WO2024225472A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026163542A1 (ja) * 2025-01-29 2026-08-06 株式会社日本触媒 感光性組成物、硬化物、積層フィルム及び物品

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2026132042A (ja) * 2025-02-04 2026-08-17 デクセリアルズ株式会社 光学積層体、物品及び光学積層体の製造方法

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2019164255A (ja) * 2018-03-20 2019-09-26 株式会社ダイセル 反射防止フィルム
JP2019214670A (ja) * 2018-06-12 2019-12-19 東レコーテックス株式会社 光硬化型プラスチック基板用ハードコート組成物およびハードコート塗膜
JP2021134303A (ja) * 2020-02-28 2021-09-13 アイカ工業株式会社 ハードコート樹脂及びハードコートフィルム
JP2022007992A (ja) * 2020-03-04 2022-01-13 デクセリアルズ株式会社 光学積層体、物品、光学積層体の製造方法

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR102056113B1 (ko) 2015-04-10 2019-12-16 후지필름 가부시키가이샤 투명 필름, 편광판, 및 화상 표시 장치
JP6825825B2 (ja) * 2015-05-27 2021-02-03 デクセリアルズ株式会社 積層薄膜、及び積層薄膜の製造方法
JP2022185597A (ja) 2019-10-31 2022-12-15 クミアイ化学工業株式会社 アゾール誘導体及びその用途
JP7190458B2 (ja) 2020-01-08 2022-12-15 株式会社ダイセル 反射防止フィルム

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2019164255A (ja) * 2018-03-20 2019-09-26 株式会社ダイセル 反射防止フィルム
JP2019214670A (ja) * 2018-06-12 2019-12-19 東レコーテックス株式会社 光硬化型プラスチック基板用ハードコート組成物およびハードコート塗膜
JP2021134303A (ja) * 2020-02-28 2021-09-13 アイカ工業株式会社 ハードコート樹脂及びハードコートフィルム
JP2022007992A (ja) * 2020-03-04 2022-01-13 デクセリアルズ株式会社 光学積層体、物品、光学積層体の製造方法

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026163542A1 (ja) * 2025-01-29 2026-08-06 株式会社日本触媒 感光性組成物、硬化物、積層フィルム及び物品

Also Published As

Publication number Publication date
CN121002404A (zh) 2025-11-21
JP2024159608A (ja) 2024-11-08
JP7850197B2 (ja) 2026-04-22
KR20250168355A (ko) 2025-12-02
JP2026034585A (ja) 2026-02-27

Similar Documents

Publication Publication Date Title
US12455403B2 (en) Optical laminate, article and method of manufacturing optical laminate
JP7688609B2 (ja) 光学積層体、物品、光学積層体の製造方法
JP7684934B2 (ja) 光学積層体の製造方法
JP7089609B2 (ja) 光学積層体、物品、光学積層体の製造方法
JP7791853B2 (ja) 光学積層体の製造方法
KR102735288B1 (ko) 광학 적층체, 물품, 광학 적층체의 제조 방법
JP7824911B2 (ja) 光学積層体の製造方法
JP2025179201A (ja) 光学積層体、物品および画像表示装置
JP2026034585A (ja) 光学積層体及びこれを備えた物品
KR102823789B1 (ko) 광학 적층체의 제조 방법
JP7134373B1 (ja) 光学積層体、物品および画像表示装置
TW202216458A (zh) 光學積層體之製造方法
US20260299171A1 (en) Optical laminate and article provided with same
JP7241949B1 (ja) 光学積層体、物品および画像表示装置
JP2026078098A (ja) 光学積層体及びこれを備えた物品
TW202448692A (zh) 光學積層體及具備其之物品
JP2022060214A (ja) 光学積層体の製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24797214

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 1020257034507

Country of ref document: KR

Free format text: ST27 STATUS EVENT CODE: A-0-1-A10-A15-NAP-PA0105 (AS PROVIDED BY THE NATIONAL OFFICE)

WWE Wipo information: entry into national phase

Ref document number: KR1020257034507

Country of ref document: KR

Ref document number: 1020257034507

Country of ref document: KR

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 1020257034507

Country of ref document: KR

122 Ep: pct application non-entry in european phase

Ref document number: 24797214

Country of ref document: EP

Kind code of ref document: A1