WO2023218949A1 - シリカ粒子分散液 - Google Patents

シリカ粒子分散液 Download PDF

Info

Publication number
WO2023218949A1
WO2023218949A1 PCT/JP2023/016364 JP2023016364W WO2023218949A1 WO 2023218949 A1 WO2023218949 A1 WO 2023218949A1 JP 2023016364 W JP2023016364 W JP 2023016364W WO 2023218949 A1 WO2023218949 A1 WO 2023218949A1
Authority
WO
WIPO (PCT)
Prior art keywords
silica particles
particle dispersion
spherical silica
mass
silica particle
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/016364
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
博道 加茂
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
AGC Si Tech Co Ltd
AGC Inc
Original Assignee
Asahi Glass Co Ltd
AGC Si Tech Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Asahi Glass Co Ltd, AGC Si Tech Co Ltd filed Critical Asahi Glass Co Ltd
Priority to CN202380038964.2A priority Critical patent/CN119156348A/zh
Priority to KR1020247036876A priority patent/KR20250008054A/ko
Priority to JP2024520371A priority patent/JPWO2023218949A1/ja
Publication of WO2023218949A1 publication Critical patent/WO2023218949A1/ja
Priority to US18/938,403 priority patent/US20250059355A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
    • C01B33/00—Silicon; Compounds thereof
    • C01B33/113—Silicon oxides; Hydrates thereof
    • C01B33/12—Silica; Hydrates thereof, e.g. lepidoic silicic acid
    • C01B33/14—Colloidal silica, e.g. dispersions, gels, sols
    • C01B33/145—Preparation of hydroorganosols, organosols or dispersions in an organic medium
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09C—TREATMENT OF INORGANIC MATERIALS, OTHER THAN FIBROUS FILLERS, TO ENHANCE THEIR PIGMENTING OR FILLING PROPERTIES ; PREPARATION OF CARBON BLACK  ; PREPARATION OF INORGANIC MATERIALS WHICH ARE NO SINGLE CHEMICAL COMPOUNDS AND WHICH ARE MAINLY USED AS PIGMENTS OR FILLERS
    • C09C1/00—Treatment of specific inorganic materials other than fibrous fillers; Preparation of carbon black
    • C09C1/28—Compounds of silicon
    • C09C1/30—Silicic acid
    • C09C1/3072—Treatment with macro-molecular organic compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/34—Silicon-containing compounds
    • C08K3/36—Silica
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K7/00—Use of ingredients characterised by shape
    • C08K7/16—Solid spheres
    • C08K7/18—Solid spheres inorganic
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K7/00—Use of ingredients characterised by shape
    • C08K7/22—Expanded, porous or hollow particles
    • C08K7/24—Expanded, porous or hollow particles inorganic
    • C08K7/26—Silicon- containing compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K9/00—Use of pretreated ingredients
    • C08K9/04—Ingredients treated with organic substances
    • C08K9/06—Ingredients treated with organic substances with silicon-containing compounds
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09C—TREATMENT OF INORGANIC MATERIALS, OTHER THAN FIBROUS FILLERS, TO ENHANCE THEIR PIGMENTING OR FILLING PROPERTIES ; PREPARATION OF CARBON BLACK  ; PREPARATION OF INORGANIC MATERIALS WHICH ARE NO SINGLE CHEMICAL COMPOUNDS AND WHICH ARE MAINLY USED AS PIGMENTS OR FILLERS
    • C09C1/00—Treatment of specific inorganic materials other than fibrous fillers; Preparation of carbon black
    • C09C1/28—Compounds of silicon
    • C09C1/30—Silicic acid
    • C09C1/3009—Physical treatment, e.g. grinding; treatment with ultrasonic vibrations
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09C—TREATMENT OF INORGANIC MATERIALS, OTHER THAN FIBROUS FILLERS, TO ENHANCE THEIR PIGMENTING OR FILLING PROPERTIES ; PREPARATION OF CARBON BLACK  ; PREPARATION OF INORGANIC MATERIALS WHICH ARE NO SINGLE CHEMICAL COMPOUNDS AND WHICH ARE MAINLY USED AS PIGMENTS OR FILLERS
    • C09C1/00—Treatment of specific inorganic materials other than fibrous fillers; Preparation of carbon black
    • C09C1/28—Compounds of silicon
    • C09C1/30—Silicic acid
    • C09C1/3081—Treatment with organo-silicon compounds
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D17/00—Pigment pastes, e.g. for mixing in paints
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/30—Particle morphology extending in three dimensions
    • C01P2004/32—Spheres
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/60—Particles characterised by their size
    • C01P2004/61—Micrometer sized, i.e. from 1-100 micrometer
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/60—Particles characterised by their size
    • C01P2004/62—Submicrometer sized, i.e. from 0.1-1 micrometer
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/12—Surface area
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/22—Rheological behaviour as dispersion, e.g. viscosity, sedimentation stability
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/002—Physical properties
    • C08K2201/005—Additives being defined by their particle size in general
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/002—Physical properties
    • C08K2201/006—Additives being defined by their surface area

Definitions

  • the present invention relates to a silica particle dispersion in which silica particles are dispersed in a solvent.
  • Silica particles have traditionally been used in a variety of applications, including electronic materials such as printed wiring boards and package wiring boards, optical materials such as lenses and optical films, functional materials such as catalysts and catalyst carriers, and pigments for paints and cosmetics. ing.
  • silica particles have been utilized in electronic substrates by taking advantage of their low dielectric properties.
  • Silica particles tend to aggregate when used in the dry powder state, so depending on the purpose of use, they are used in the form of a dispersion in a solvent such as water or resin.
  • a solvent such as water or resin.
  • Patent Document 1 states that the particle size is 100 nm to 2000 nm or the specific surface area is 2 m 2 /g to 35 m 2 /g, and the amount of water generated when heated at 200°C is 40 ppm per 1 m 2 of surface area.
  • a filler for electronic materials which is a silica particle material whose surface is treated with a silane compound having a vinyl group, a phenyl group, a phenylamino group, an alkyl group having 4 or more carbon atoms, a methacrylic group, or an epoxy group;
  • a slurry for electronic materials including a liquid dispersion medium that does not substantially contain water has been proposed.
  • Patent Document 2 describes silica-based hollow fine particles (A) having an average particle diameter (Dpa) in the range of 30 to 200 nm, and silica solid fine particles (B) having an average particle diameter (Dpb) in the range of 5 to 80 nm.
  • concentration (CA) of the silica-based hollow particles (A) is in the range of 0.2 to 8% by weight as a solid content
  • concentration (CB) of the silica solid particles (B) is 0.2 to 8% by weight as a solid content.
  • a coating liquid for forming an anti-reflection film having a weight ratio (B/A) of silica-based hollow fine particles (A) to silica solid fine particles (B) of 0.25 to 4, which is in the range of 2 to 8% by weight. is proposed.
  • Patent Document 3 describes silica-based particles having an average particle diameter of 5 to 40 nm and a ratio of the number of hollow particles to the total number of hollow particles and solid particles (hollowness ratio) of 70% or more. Dispersions of silica-based particles have been proposed.
  • silica particle dispersions when conventional silica particle dispersions are incorporated into a resin composition and formed into a film, the silica particles tend to clump, resulting in low peel strength, and it is sometimes difficult to obtain the expected effects of silica particles.
  • Ta Particularly when using the silica particles for the purpose of lowering the dielectricity, lowering the dielectricity can be achieved by reducing the surface area of the silica particles or increasing the particle size, but this tends to reduce peel strength because the contact area between the particles increases. .
  • the present invention has been made in view of the above-mentioned problems, and an object thereof is to provide a silica particle dispersion liquid that can suppress grain formation during film formation and increase peel strength.
  • the present invention relates to the following (1) to (9).
  • (1) Contains spherical silica particles and a solvent, the median diameter d50 of the spherical silica particles is 0.5 to 20 ⁇ m, and the specific surface area A (m 2 /g) of the spherical silica particles and the median diameter d50 ( ⁇ m)
  • the silica particle dispersion was dried to obtain powdered spherical silica particles, and 8 parts by mass of the obtained powdered spherical silica particles and 6 parts by mass of boiled linseed oil were mixed and kneaded at 2000 rpm for 3 minutes. The kneaded material was measured using a rotary rheometer at a shear rate of 1 s -1 for 30 seconds, and the viscosity at 30 seconds was determined.
  • the above (1) further contains a silane compound having at least one group selected from the group consisting of a vinyl group, a phenyl group, a phenylamino group, an alkyl group having 4 or more carbon atoms, a methacryl group, and an epoxy group.
  • the solvent includes at least one selected from the group consisting of water, hydrocarbons, alcohols, acetic esters, ketones, cellosolves, glycol ethers, chlorinated hydrocarbons, and polar solvents.
  • the solvent has a median diameter d50 of 0.5 to 20 ⁇ m, and the product A ⁇ d50 of the specific surface area A (m 2 /g) and the median diameter d50 ( ⁇ m) is 2.7 to 5.0 ⁇ m ⁇ m 2 /g of spherical silica particles, the mixed liquid is subjected to a dispersion treatment, and the aggregates of the spherical silica particles are removed by classification.
  • silica particle dispersion of the present invention spherical silica particles are uniformly dispersed in the liquid without agglomeration, so grain formation is suppressed when a resin composition containing the silica particle dispersion of the present invention is formed into a film. It also increases the peel strength.
  • the silica particle dispersion of the present invention contains spherical silica particles and a solvent, the spherical silica particles have a median diameter d50 of 0.5 to 20 ⁇ m, and have a specific surface area A (m 2 /g) and a median diameter d50 ( ⁇ m).
  • the product A ⁇ d50 is 2.7 to 5.0 ⁇ m ⁇ m 2 /g.
  • the spherical silica particles are uniformly dispersed without agglomeration, and the dispersion stability of the spherical silica particles in the dispersion is improved. It is possible to suppress grain formation during peeling and increase peel strength.
  • the solvent used as the dispersion medium for the silica particle dispersion can be arbitrarily selected depending on the purpose of use, and examples include water, hydrocarbons, alcohols, acetate esters, ketones, cellosolves, glycol ethers, and chlorinated hydrocarbons. and polar solvents.
  • the solvent contains at least one selected from the group consisting of these.
  • hydrocarbons examples include toluene, methylcyclohexane, normal heptane, m-xylene, and the like.
  • alcohols include ethanol, isopropyl alcohol, 1-propyl alcohol, isobutyl alcohol, 1-butanol, 2-butanol, and the like.
  • acetic acid esters include propyl acetate, isobutyl acetate, butyl acetate, and the like.
  • ketones examples include methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
  • cellosolves include ethylene glycol monomethyl ether and ethylene glycol monoethyl ether.
  • glycol ethers examples include 1-methoxy-2-propanol, 1-methoxypropyl-2-acetate, 1-ethoxy-2-propanol, and ethyl 3-ethoxypropionate.
  • chlorinated hydrocarbons examples include trichlorethylene and tetrachloroethylene.
  • the polar solvent examples include N-methyl-2-pyrrolidone.
  • the solvent may be appropriately selected depending on the intended field of use.
  • ketones and hydrocarbons it is preferable to use ketones and hydrocarbons, and specifically, it is preferable to use methyl ethyl ketone (MEK), toluene, etc.
  • MEK methyl ethyl ketone
  • the liquid main ingredient or curing agent itself may be used as a solvent.
  • the base resin include epoxy resins, polyphenylene ether resins, polyester resins, polyimide resins, phenol resins, ortho-divinylbenzene resins
  • the curing agent include polyamine-based curing agents and acid anhydride-based curing agents. , phenolic curing agents, active ester curing agents, peroxides, and the like.
  • the solvent is preferably contained in the silica particle dispersion in an amount of 15 to 90% by mass.
  • the content of the solvent is 15% by mass or more, the spherical silica particles can be uniformly dispersed, and the viscosity of the dispersion liquid does not become too high, making it easy to handle.
  • the content of the solvent is 90% by mass or less, it is liquid and can be used in a dispersed state.
  • the content of the solvent in the silica particle dispersion is more preferably 20% by mass or more, further preferably 25% by mass or more, particularly preferably 30% by mass or more, most preferably 40% by mass or more, and 85% by mass or more. It is more preferably at most 80% by mass, even more preferably at most 75% by mass.
  • the spherical silica particles are solid silica, have a median diameter d50 of 0.5 to 20 ⁇ m, and have a product A x d50 of specific surface area A (m 2 /g) and median diameter d50 ( ⁇ m) of 2.7 to 20. It is in the range of 5.0 ⁇ m ⁇ m 2 /g (2.7 ⁇ A ⁇ d50 ( ⁇ m ⁇ m 2 /g) ⁇ 5.0).
  • the physical properties of the spherical silica particles described below can be confirmed by drying a silica particle dispersion to obtain powdery silica particles.
  • the median diameter d50 of the spherical silica particles is within the above range, the viscosity is easy to handle and grains do not easily stand during coating, so the peel strength of the resin composition is maintained appropriately when used as a resin composition.
  • the median diameter d50 of the spherical silica particles is in the range of 0.5 to 20 ⁇ m.
  • the median diameter d50 is preferably 1 ⁇ m or more, and the upper limit is preferably 10 ⁇ m or less, more preferably 5 ⁇ m or less.
  • the median diameter d50 is determined by a laser diffraction type particle size distribution measuring device (for example, "MT3300EXII” manufactured by Microtrac Bell Co., Ltd.).
  • the specific surface area A of the spherical silica particles is preferably in the range of 0.1 to 10 m 2 /g.
  • the specific surface area A is more preferably 8 m 2 /g or less, even more preferably 7 m 2 /g or less, particularly preferably 5 m 2 /g or less. Note that it is substantially difficult to obtain a material with a specific surface area A of less than 0.1 m 2 /g.
  • the specific surface area was determined by the BET method based on the nitrogen adsorption method using a specific surface area/pore distribution measuring device (for example, Microtrac BEL SORP-mini II, Micromeritic TriStar II, etc.). demand.
  • a specific surface area/pore distribution measuring device for example, Microtrac BEL SORP-mini II, Micromeritic TriStar II, etc.
  • the product A ⁇ d50 of the specific surface area A (m 2 /g) and median diameter d50 ( ⁇ m) of the spherical silica particles is 2.7 to 5.0 ⁇ m ⁇ m 2 /g, preferably 2.7 to 4 .5 ⁇ m ⁇ m 2 /g, more preferably 2.7 to 4.0 ⁇ m ⁇ m 2 /g.
  • the value of A ⁇ d50 is 5.0 ⁇ m ⁇ m 2 /g or less, the specific surface area per particle size becomes small, and the dielectric loss tangent can be made small.
  • the sphericity of the spherical silica particles is preferably 0.75 to 1.0. If the sphericity becomes too low, the contact area of the silica particles in the resin layer with the member in contact with the resin composition containing the silica particle dispersion may decrease, resulting in a decrease in peel strength. is preferably 0.75 or more.
  • Sphericity is defined as the maximum diameter (DL) of any 100 particles in a photographic projection obtained by photographing with a scanning electron microscope (SEM), and the short diameter (DS) perpendicular to this. can be expressed as an average value obtained by measuring the ratio of the minimum diameter (DS) to the maximum diameter (DL) (DS/DL). From the viewpoint of dispersibility, etc., the sphericity is more preferably 0.90 or more, even more preferably 0.93 or more, and the closer to 1.0, the more preferable it is.
  • the spherical silica particles have a viscosity of 5000 mPa ⁇ s or less as measured by the following measuring method.
  • the silica particle dispersion was dried to obtain powdered spherical silica particles, and 8 parts by mass of the obtained powdered spherical silica particles and 6 parts by mass of boiled linseed oil were mixed and kneaded at 2000 rpm for 3 minutes.
  • the kneaded material is measured using a rotary rheometer at a shear rate of 1 s -1 for 30 seconds, and the viscosity at 30 seconds is determined.
  • the viscosity of the kneaded product at a shear rate of 1 s ⁇ 1 determined by the above measurement method is 5000 mPa ⁇ s or less, it can be said that the silica particles are dense, and the peel strength when made into a resin composition can be improved. Furthermore, the amount of solvent added during molding and film formation of a resin composition containing spherical silica particles can be reduced, drying speed can be increased, and productivity can be improved. In addition, when the specific surface area of silica particles increases depending on the particle size, the viscosity tends to increase when added to a resin composition, but spherical silica particles have a small specific surface area and therefore suppress the increase in viscosity of the resin composition. can.
  • the viscosity of the kneaded material is more preferably 4000 mPa ⁇ s or less, and even more preferably 3500 mPa ⁇ s or less.
  • the lower limit of the viscosity of the kneaded product at a shear rate of 1 s -1 is not particularly limited because the lower the viscosity, the better the coating properties of the resin composition and the higher the productivity.
  • the dielectric loss tangent of the spherical silica particles as a powder is preferably 0.0020 or less at a frequency of 1 GHz, more preferably 0.0010 or less, and even more preferably 0.0008 or less. Particularly in the measurement of the dielectric loss tangent and dielectric constant of powder, the sample space becomes smaller and the measurement accuracy deteriorates at frequencies of 10 GHz or more, so in the present invention, measured values at a frequency of 1 GHz are used.
  • the dielectric loss tangent of the spherical silica particles at a frequency of 1 GHz is 0.0020 or less, an excellent dielectric loss suppressing effect can be obtained, so that a substrate or sheet with improved high frequency characteristics can be obtained.
  • the smaller the dielectric loss tangent, the more suppressed the transmission loss of the circuit, so the lower limit is not particularly limited.
  • the dielectric loss tangent can be measured using a perturbation resonator method using a dedicated device (for example, "Vector Network Analyzer E5063A” manufactured by Keycom Co., Ltd.).
  • the IR peak intensity near 3746 cm ⁇ 1 derived from isolated silanol groups on the surface of the spherical silica particles is preferably 0.1 or less, more preferably 0.08 or less, and even more preferably 0.06 or less.
  • An isolated silanol group is a silanol (Si-OH) group that is not bonded to water or the like adsorbed on silica particles.
  • the amount of isolated silanol (Si-OH) groups on the surface of silica particles can be obtained by IR measurement. Specifically, after normalizing the IR spectrum at 800 cm ⁇ 1 and aligning the baseline at 3800 cm ⁇ 1 , the relative value of the Si—OH peak intensity around 3746 cm ⁇ 1 is determined.
  • dielectric loss tends to increase when a member mixed with resin is used for electronic purposes, but the IR peak intensity near 3746 cm -1 derived from the isolated silanol groups on the particle surface is 0.1 or less, dielectric loss can be reduced.
  • the maximum IR peak intensity at 3300 to 3700 cm ⁇ 1 derived from bonded silanol groups on the surface of the spherical silica particles is preferably 0.2 or less, more preferably 0.17 or less, and 0.15 or less. More preferred.
  • the bonded silanol group is a silanol (Si-OH) group that is bonded to water adsorbed on silica particles, silanol, etc. on the silica surface.
  • the amount of bound silanol (Si-OH) groups on the surface of silica particles can be obtained by IR measurement.
  • the relative value of the combined Si-OH peak intensity is determined from the maximum peak between 3300 and 3700 cm -1 . . If there are many bonded silanol groups on the particle surface, the dielectric loss tends to increase when the material mixed with the resin is used for electronic purposes. When the maximum IR peak intensity is 0.2 or less, dielectric loss can be reduced.
  • the spherical silica particles are preferably non-porous particles. If the particles are porous, the oil absorption will increase, the viscosity in the resin will increase, the surface area will increase, the amount of silanol (Si-OH) groups on the surface of the silica particles will increase, and the dielectric loss tangent will increase. It tends to get worse.
  • the oil absorption amount is preferably 100 ml/100 g or less, more preferably 70 ml/100 g or less, and most preferably 50 ml/100 g or less. Although the lower limit is not particularly limited, it is substantially difficult to reduce the oil absorption amount to 20 ml/100 g or less.
  • the spherical silica particles preferably contain titanium (Ti) in a range of 30 to 1500 ppm, more preferably 100 to 1000 ppm, and still more preferably 100 to 500 ppm.
  • Ti is a component that is optionally included in the production of spherical silica particles.
  • Ti is a component that is optionally included in the production of spherical silica particles.
  • the fine powder will adhere to the surface of the base particles, increasing the specific surface area of the particles.
  • thermal compaction becomes easier during firing.
  • the spherical silica particles may contain impurity elements other than titanium (Ti) within a range that does not impede the effects of the present invention.
  • impurity elements include, for example, Na, K, Mg, Ca, Al, Fe, and the like.
  • the total content of alkali metals and alkaline earth metals among the impurity elements is preferably 2000 ppm or less, more preferably 1000 ppm or less, and even more preferably 200 ppm or less.
  • the spherical silica particles may be treated with a silane coupling agent.
  • a silane coupling agent By treating the surface of the spherical silica particles with a silane coupling agent, the amount of residual silanol groups on the surface is reduced, making the surface hydrophobic, suppressing moisture adsorption, improving dielectric loss, and improving the ability of resin compositions. In this case, the affinity with the resin is improved, and the dispersibility and strength after resin film formation are improved.
  • surface treatment conditions there are no particular restrictions on the surface treatment conditions, and general surface treatment conditions may be used, and a wet treatment method or a dry treatment method can be used. From the viewpoint of uniform treatment, a wet treatment method is preferred.
  • silane coupling agents include aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, organosilazane compounds, and the like.
  • One type of silane coupling agent may be used alone, or two or more types may be used in combination.
  • examples of the silane coupling agent include aminopropylmethoxysilane, aminopropyltriethoxysilane, ureidopropyltriethoxysilane, N-phenylaminopropyltrimethoxysilane, N-2 (aminoethyl)aminopropyltrimethoxysilane, etc.
  • aminosilane coupling agent glycidoxypropyltrimethoxysilane, glycidoxypropyltriethoxysilane, glycidoxypropylmethyldiethoxysilane, glycidylbutyltrimethoxysilane, (3,4-epoxycyclohexyl)ethyltrimethoxysilane
  • Epoxysilane coupling agents such as mercaptopropyltrimethoxysilane, mercaptosilane coupling agents such as mercaptopropyltriethoxysilane, methyltrimethoxysilane, vinyltrimethoxysilane, octadecyltrimethoxysilane, phenyltrimethoxysilane, meth Silane coupling agents such as chloropropyltrimethoxysilane, imidazolesilane , and triazinesilane , CF3 ( CF2 ) 7CH2CH2Si
  • the amount of the silane coupling agent attached is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, and still more preferably 0.10 parts by mass or more, based on 100 parts by mass of spherical silica particles. It is preferably 5 parts by mass or less, and even more preferably 2 parts by mass or less.
  • the surface of the spherical silica particles has been treated with the silane coupling agent by detecting a peak due to the substituent of the silane coupling agent using IR. Further, the amount of attached silane coupling agent can be measured by the amount of carbon.
  • the spherical silica particles are preferably contained in a range of 10 to 85% by mass in the silica particle dispersion.
  • the content of spherical silica particles is 10% by mass or more, the desired peel strength can be imparted with a small amount of silica particle dispersion added to the resin composition, and when the content is 85% by mass or less, the viscosity of the dispersion is low. It does not rise too much and is easy to handle.
  • the content of spherical silica particles in the silica particle dispersion is more preferably 15% by mass or more, even more preferably 20% by mass or more, particularly preferably 25% by mass or more, and 80% by mass or less. is more preferred, 75% by mass or less is even more preferred, particularly preferably 70% by mass or less, and most preferably 60% by mass or less.
  • the silica particle dispersion of the present invention contains a silane compound having at least one group selected from the group consisting of vinyl group, phenyl group, phenylamino group, alkyl group having 4 or more carbon atoms, methacrylic group, and epoxy group. It is preferable to do so.
  • a silane compound having at least one group selected from the group consisting of vinyl group, phenyl group, phenylamino group, alkyl group having 4 or more carbon atoms, methacrylic group, and epoxy group. It is preferable to do so.
  • the silane compound when the silica particle dispersion is included in the resin composition, the surface of the spherical silica particles blends into the resin, so that the peel strength of the resin composition can be further increased. Note that when the spherical silica particles are treated with a silane coupling agent, it is not necessary to add a silane compound.
  • silane compound examples include vinylsilane, phenylsilane, phenylaminosilane, hexylsilane, decylsilane, 3-methacryloxypropyltrimethoxysilane, and aminopropylsilane. These may be used alone or in combination of two or more. Among these, from the viewpoint of interaction with the resin, silane compounds containing a vinyl group, phenyl group, methacrylic group, epoxy group or phenylamino group are preferable, and silane compounds containing a vinyl group, phenyl group, methacrylic group or phenylamino group are preferable. More preferred are silane compounds containing a phenyl group or a methacrylic group.
  • the dispersibility of the silica particles in the kneaded product described below or the silica particle dispersion of the present invention is improved, and the viscosity thereof and the peel strength of the molded product formed therefrom are particularly easy to maintain a balance.
  • the silane compound is preferably contained in the silica particle dispersion in a range of 0.01 to 5% by mass.
  • the content of the silane compound is 0.01% by mass or more, when the silica particle dispersion is included in the resin composition, the compatibility between the spherical silica particles and the resin is increased, and the peel strength of the resin composition is increased. If the amount is 5% by mass or less, it can be suppressed from remaining in the composition and the influence on the physical properties of the resin composition can be reduced.
  • the content of the silane compound in the silica particle dispersion is more preferably 0.02% by mass or more, further preferably 0.04% by mass or more, particularly preferably 0.05% by mass or more, and 4% by mass. It is more preferably at most 3% by mass, particularly preferably at most 3% by mass.
  • the silica particle dispersion of the present invention preferably further contains an organic thixotropic agent.
  • the organic thixotropic agent is used to suppress agglomeration and precipitation of spherical silica particles in a silica particle dispersion and a resin composition or slurry containing the silica particle dispersion, and to prevent flux from wetting the cured product of the resin composition or slurry. Added to improve sex.
  • organic thixotropic agents include fatty acid amides (amide wax type) synthesized from vegetable oil fatty acids and amines; surfactant types such as fatty acid esters, polyethers, sulfated oils, and higher alcohol sulfates; polycarbonate. Acid esters; polycarboxylic acid amides; urea-modified compounds are included, but hydrogenated castor oil-based ones called castor oil waxes, and oxidized polyethylene-based waxes that are made by oxidizing polyethylene and introducing polar groups. Not included.
  • One type of organic thixotropic agent may be used alone, or two or more types may be used in combination.
  • Organic thixotropic agents are commercially available, such as BYK®-R606, BYK®-405, BYK®-R605, BYK®-R607, BYK® )-410, BYK (registered trademark) -411, BYK (registered trademark) -415, BYK (registered trademark) -430, BYK (registered trademark) -431, BYK (registered trademark) -7410ET, BYK (registered trademark) - 7411ES (manufactured by BIC Chemie Japan), Talen 1450, Talen 2000, Talen 2200A, Talen 7200-20, Talen 8200-20, Talen 8300-20, Talen 8700-20, Talen BA-600, Flownon SH-290, Examples include Fluonon SH-295S, Fluonon SH-350, Fluonon HR-2, and Fluonon HR-4AF (manufactured by Kyoeisha Kagaku Co., Ltd.).
  • the organic thixotropic agent is preferably contained in the silica particle dispersion in a range of 0.01 to 5% by mass.
  • the content of the organic thixotropic agent is 0.01% by mass or more, the aggregation of spherical silica particles in the dispersion is suppressed, and when the silica particle dispersion is included in the resin composition, there are It can prevent resin from accumulating. This increases the peel strength of the resin composition.
  • the content of the organic thixotropic agent is 5% by mass or less, it is possible to suppress the organic thixotropic agent from remaining in the composition, thereby reducing the influence on the physical properties of the resin composition.
  • the content of the organic thixotropic agent in the silica particle dispersion is more preferably 0.02% by mass or more, further preferably 0.04% by mass or more, particularly preferably 0.05% by mass or more, and 4% by mass or more. It is more preferably at most 3% by mass, even more preferably at most 2.5% by mass, and particularly preferably at most 2.5% by mass.
  • the silica particle dispersion of the present invention may contain other optional components within a range that does not impair the effects of the present invention.
  • optional components include other inorganic fillers such as alumina, hardening compositions, and the like.
  • the silica particle dispersion of the present invention preferably has a viscosity of 20 to 20,000 mPa ⁇ s at 25° C. when the solid content concentration of the spherical silica particles is 70% by mass. If the viscosity at 25°C of a silica particle dispersion with a solid content concentration of spherical silica particles of 50% by mass is 20 mPa ⁇ s or more, sedimentation (floating) separation of silica can be prevented, and if it is 20000 mPa ⁇ s or less, silica dispersion can be prevented. It can be used while maintaining its condition.
  • the viscosity is more preferably 50 mPa ⁇ s or more, even more preferably 75 mPa ⁇ s or more, particularly preferably 100 mPa ⁇ s or more, and most preferably 500 mPa ⁇ s or more. Further, it is more preferably 15,000 mPa ⁇ s or less, even more preferably 12,000 mPa ⁇ s or less, and particularly preferably 10,000 mPa ⁇ s or less.
  • the silica particle dispersion of the present invention is obtained by dispersing spherical silica particle powder in a solvent.
  • the spherical silica particles may be obtained by manufacturing, or commercially available spherical silica particles may be used.
  • a method for producing spherical silica particles and a method for producing a silica particle dispersion using the same will be explained.
  • Method for producing spherical silica particles examples include a method in which a spherical silica precursor is formed by a wet method and spherical silica particles are obtained from this precursor.
  • the wet method refers to a method including a step of using a liquid silica source and gelling it to obtain a raw material for spherical silica particles.
  • spherical silica particles can be formed, so there is no need to adjust the shape of the particles by pulverization or the like, and as a result, particles with a small specific surface area can be obtained.
  • the wet method particles that are significantly smaller than the average particle diameter are difficult to produce, and the specific surface area tends to become small after firing. Furthermore, in the wet method, by adjusting the impurities in the silica source, the amount of impurity elements such as titanium can be adjusted, and furthermore, the above-mentioned impurity elements can be uniformly dispersed in the particles.
  • Examples of the wet method include a spray method, an emulsion gelling method, and the like.
  • an emulsion gelling method for example, a dispersed phase containing a silica precursor and a continuous phase are emulsified, and the resulting emulsion is gelled to obtain a spherical silica precursor.
  • the emulsification method it is preferable to prepare an emulsion by supplying a dispersed phase containing a silica precursor to a continuous phase through micropores or a porous membrane. In this way, an emulsion with a uniform droplet size is produced, and as a result, spherical silica with a uniform particle size is obtained.
  • a micromixer method or a membrane emulsification method is used.
  • the micromixer method is disclosed in International Publication No. 2013/062105.
  • the pore volume of the spherical silica precursor obtained by the wet method is preferably 0.3 to 2.2 ml/g. If the pore volume of the silica precursor is 0.3 ml/g or more, the silica particles will sufficiently shrink during firing, making it possible to reduce the specific surface area.
  • the pore volume of the silica precursor is preferably 0.3 ml/g or more, more preferably 0.6 ml/g or more, and even more preferably 0.7 ml/g or more.
  • the pore volume of the silica precursor is 2.2 ml/g or less, it is possible to suppress the bulk density before firing from becoming too large and improve productivity.
  • the pore volume of the silica precursor is preferably 2.2 ml/g or less, more preferably 1.8 ml/g or less, and most preferably 1.5 ml/g or less.
  • the pore volume is determined by the BJH method based on the nitrogen adsorption method using a specific surface area/pore distribution measuring device (for example, Microtrac BEL SORP-mini II, Micromeritic TriStar II, etc.). Find it by a specific surface area/pore distribution measuring device (for example, Microtrac BEL SORP-mini II, Micromeritic TriStar II, etc.). Find it by a specific surface area/pore distribution measuring device (for example, Microtrac BEL SORP-mini II, Micromeritic TriStar II, etc.). Find it by a specific surface area/pore distribution measuring device.
  • the ignition loss of the silica precursor obtained by the wet method is preferably 5.0 to 15.0% by mass.
  • the ignition loss is the sum of adhering water attached to the silica precursor and water generated by condensation of the silanol groups contained in the silica precursor, and it is important that the silica precursor has an appropriate amount of silanol groups.
  • condensation progresses and the number of silanol groups tends to decrease. If the loss on ignition is too large, the yield during calcination will decrease and productivity will deteriorate, so the loss on ignition of the silica precursor is preferably 15.0% by mass or less, and 13.0% by mass or less. It is more preferably 12.0% by mass or less, and most preferably 12.0% by mass or less.
  • the loss on ignition of the silica precursor is preferably 5.0% by mass or more, more preferably 6.0% by mass or more, and 7.0% by mass. % or more is most preferable.
  • the ignition loss is determined as the mass loss when 1 g of the silica precursor is heated and dried at 850° C. for 0.5 hours in accordance with JIS K0067.
  • Spherical silica particles are obtained by heat-treating the spherical silica precursor.
  • the spherical silica particles are sintered to densify the shell, reduce the amount of silanol groups on the surface, and lower the dielectric loss tangent.
  • the temperature of the heat treatment is preferably 700°C or higher, more preferably 800°C or higher, and most preferably 900°C or higher.
  • the temperature is preferably 1600°C or lower, more preferably 1500°C or lower, and most preferably 1400°C or lower. That is, it is preferable to perform heat treatment in the range of 700 to 1600°C.
  • the method of the heat treatment is not particularly limited, but examples include heat treatment by a stationary method, heat treatment by a rotary kiln method, heat treatment by spray combustion, and the like.
  • the spherical silica particles obtained in the above process may be aggregated due to the drying or firing process, so they may be crushed to make the aggregate size easier to handle, but in the present invention, they may be mixed with the solvent as is.
  • a silica particle dispersion can be obtained. Examples of crushing methods include using a mortar, dry or wet ball mill, shaking sieve, and crushing machines such as pin mills, cutter mills, hammer mills, knife mills, roller mills, and jet mills. There are ways to use .
  • the obtained spherical silica particles are mixed with a solvent to obtain a silica particle dispersion.
  • the method for producing a silica particle dispersion of the present invention includes mixing a solvent and powder of spherical silica particles, dispersing the mixed liquid, and classifying the mixture to remove aggregates of spherical silica particles.
  • the spherical silica particles have a median diameter d50 of 0.5 to 20 ⁇ m, and a product A ⁇ d50 of specific surface area A (m 2 /g) and median diameter d50 ( ⁇ m) of 2.7 to 5.0 ⁇ m ⁇ m 2 / g.
  • the type and amount of solvent used, and other physical properties of the spherical silica particles are as described above.
  • the spherical silica particle powder is preferably mixed in the silica particle dispersion at a ratio of 10 to 85% by mass. If the proportion of spherical silica particles is too small, the productivity of the subsequent concentration step will decrease, and if it is too large, the viscosity of the silica particle dispersion may increase too much and the productivity of the dispersion treatment may decrease, so it should be 10 to 85% by mass. A range of is preferred.
  • the amount of spherical silica particles used is more preferably 15% by mass or more, even more preferably 20% by mass or more, particularly preferably 25% by mass or more, and more preferably 80% by mass or less, 75% by mass or less. % or less, particularly preferably 70% by mass or less, and most preferably 60% by mass or less.
  • a dispersion device used for pigment dispersion, etc. can be used.
  • mixers such as dispers, homomixers, and planetary mixers, homogenizers (M Technique's "Clearmix”, PRIMIX's “Filmix”, etc., Silverson's “Abramix”, etc.), paint conditioners ( Red Devil), colloid mills (PUC Colloid Mill, IKA Colloid Mill MK), corn mills (IKA Corn Mill MKO, etc.), ball mills, sand mills (Shinmaru Enterprises) "Dyno Mill” manufactured by Manufacturer Co., Ltd.), attritor, pearl mill ("DCP Mill” manufactured by Eirich Co., Ltd., etc.), media-type dispersion machines such as Koboru Mill, wet jet mill ("Ginas PY” manufactured by Genus Co., Ltd., “Starburst” manufactured by Sugino Machine Co.,
  • the temperature during the dispersion treatment is preferably 0 to 100°C.
  • the temperature during the dispersion treatment here refers to the temperature range before and after the treatment.
  • the treatment temperature is more preferably 5°C or higher, even more preferably 10°C or higher, more preferably 90°C or lower, and even more preferably 80°C or lower.
  • the time for the dispersion treatment may be set as appropriate depending on the dispersion device used to prevent particle destruction, but it is preferably 0.5 to 60 minutes, more preferably 0.5 to 10 minutes, and 0.5 to 60 minutes is preferable. .5 to 5 minutes is more preferred.
  • aggregates of spherical silica particles that remained after being unable to be dispersed even during the dispersion treatment are wet classified.
  • wet classification include classification using a sieve or centrifugal force.
  • a sieve it is preferable to classify using a sieve with an opening of 100 ⁇ m or less.
  • the sieve it is preferable to use a metal having a dense lattice structure, such as an electroformed sieve.
  • the opening of the sieve is preferably 100 ⁇ m or less, more preferably 75 ⁇ m or less, even more preferably 50 ⁇ m or less, and particularly preferably 35 ⁇ m or less. Further, the lower limit of the opening of the sieve is preferably 0.2 ⁇ m or more, more preferably 0.5 ⁇ m or more, and even more preferably 1 ⁇ m or more. That is, the opening of the sieve is preferably in the range of 0.2 to 100 ⁇ m.
  • concentration method include vaporization concentration, solid-liquid separation, and the like.
  • a silane coupling agent may be added to the mixture of the solvent and spherical silica particles.
  • the silane coupling agent include the aforementioned silane coupling agents.
  • the silica particle dispersion of the present invention can be mixed with a resin and used as a resin composition.
  • the resin composition preferably contains spherical silica particles in an amount of 5 to 70% by mass, more preferably 10 to 50% by mass.
  • resins examples include epoxy resins, silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamideimide, and polyetherimide; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide , aromatic polyester, polysulfone, liquid crystal polymer, polyether sulfone, polycarbonate, maleimide modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, polytetra One of fluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-ethylene cop
  • the resin composition may contain any components other than the above-mentioned resin and medium.
  • optional components include dispersion aids, surfactants, fillers other than silica, and the like.
  • the dielectric loss tangent thereof is preferably 0.012 or less at a frequency of 10 GHz, more preferably 0.010 or less, and still more preferably 0.009 or less. preferable.
  • the dielectric loss tangent of the resin film at a frequency of 10 GHz is 0.012 or less, it has excellent electrical properties and can be expected to be used in electronic equipment, communication equipment, etc. The smaller the dielectric loss tangent, the more suppressed the transmission loss of the circuit, so the lower limit is not particularly limited.
  • the dielectric loss tangent can be measured using a split post dielectric resonator (SPDR) (eg, manufactured by Agilent Technologies).
  • SPDR split post dielectric resonator
  • the resin film has an average linear expansion coefficient of 10 to 50 ppm/°C.
  • the average coefficient of linear expansion is more preferably 12 ppm/°C or higher, even more preferably 15 ppm/°C or higher, more preferably 40 ppm/°C or lower, even more preferably 30 ppm/°C or lower.
  • the average coefficient of linear expansion is determined by heating the above resin film at a load of 5N and a temperature increase rate of 2°C/min from 30°C using a thermomechanical analyzer (for example, "TMA-60" manufactured by Shimadzu Corporation). It is determined by measuring the dimensional change of a sample up to 150°C and calculating the average.
  • a thermomechanical analyzer for example, "TMA-60” manufactured by Shimadzu Corporation.
  • the silica particle dispersion of the present invention can be used as a variety of fillers, and is particularly used as a resin for producing electronic substrates used in electronic devices such as personal computers, notebook computers, and digital cameras, and communication devices such as smartphones and game consoles. It can be suitably used as a filler in compositions.
  • the silica particle dispersion of the present invention can be used in resin compositions, prepregs, metal foil-clad laminates, and printed wiring boards in order to reduce dielectric loss tangent, reduce transmission loss, reduce moisture absorption, and improve peel strength. It is also expected to be applied to resin sheets, adhesive layers, adhesive films, solder resists, bump reflow applications, rewiring insulating layers, die bonding materials, encapsulants, underfills, mold underfills, and laminated inductors.
  • Test Example 1 spherical silica particles were produced and a silica particle dispersion was produced using the obtained spherical silica particles.
  • spherical silica powder and 43 g of methyl ethyl ketone (MEK) were placed in a 250 ml polybottle and stirred at 30 rpm for 2 hours using a mix rotor.
  • the obtained mixed liquid was spouted three times at a pressure of 100 MPa from a ⁇ 0.1 mm nozzle using a wet atomization device (Starburst Mini manufactured by Sugino Machine Co., Ltd., model number: HJP-25001). repeated.
  • the obtained slurry was passed through an electroforming sieve with an opening of 10 ⁇ m to obtain a silica particle dispersion having a solid content of 70% by mass.
  • silica particles were A dispersion was obtained.
  • Example 5 100 g of the spherical silica powder obtained in Example 4, 43 g of methyl ethyl ketone (MEK), and 0.10 g of KBM-503 (3-methacryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were placed in a 250 ml polybottle, and a mix rotor was placed. The mixture was stirred at 30 rpm for 2 hours. The resulting mixed solution was heated at 80°C for 1 hour, cooled, and atomized using a wet atomization device (Starburst Mini manufactured by Sugino Machine Co., Ltd., model number: HJP-25001) through a ⁇ 0.1 mm nozzle. The operation of ejecting at a pressure of 100 MPa was repeated three times. The obtained slurry was passed through an electroforming sieve with an opening of 10 ⁇ m to obtain a silica particle dispersion having a solid content of 70% by mass.
  • MEK
  • Example 6 100 g of the spherical silica powder obtained in Example 4, 43 g of methyl ethyl ketone (MEK), and 0.10 g of BYK (registered trademark)-R606 (polyhydroxycarboxylic acid ester, manufactured by Big Chemie) were placed in a 250 ml polybottle, and using a mixing rotor. The mixture was stirred at 30 rpm for 2 hours. The obtained mixed liquid was spouted three times at a pressure of 100 MPa from a ⁇ 0.1 mm nozzle using a wet atomization device (Starburst Mini manufactured by Sugino Machine Co., Ltd., model number: HJP-25001). repeated. The obtained slurry was passed through an electroforming sieve with an opening of 10 ⁇ m to obtain a silica particle dispersion having a solid content of 70% by mass.
  • MEK methyl ethyl ketone
  • BYK registered trademark
  • BYK registered trademark-R606
  • Example 7 A silica particle dispersion was obtained in the same manner as in Example 5, except that 0.10 g of KBM-103 (trimethoxyphenylsilane, manufactured by Shin-Etsu Chemical Co., Ltd.) was used instead of KBM-503.
  • KBM-103 trimethoxyphenylsilane, manufactured by Shin-Etsu Chemical Co., Ltd.
  • Example 8 Spherical silica powder 5 (manufactured by Denka Corporation: FB-5D) manufactured from raw material silica manufactured by a dry method was used. 150 g of spherical silica powder 5 was filled into an alumina crucible and heat-treated at an electric furnace temperature of 1300° C. for 1 hour. After the heat treatment, the mixture was cooled to room temperature and crushed in an agate mortar to obtain spherical silica powder. A silica particle dispersion was obtained in the same manner as in Example 1 using the obtained spherical silica powder.
  • Example 9 A silica particle dispersion was obtained in the same manner as in Example 1 using spherical silica powder 6 (manufactured by Admatex: SC-04) produced from raw silica produced by the VMC method.
  • Example 10 10 g of spherical silica powder obtained in Example 4 was used as is.
  • Specific Surface Area Spherical silica particles were dried under reduced pressure at 230°C to completely remove moisture, and used as samples.
  • the specific surface area of this sample was determined by the multi-point BET method using nitrogen gas using an automatic specific surface area/pore distribution measuring device "Tristar II" manufactured by Micromeritic.
  • the median diameter was measured using a laser diffraction type particle size distribution analyzer (MT3300EXII manufactured by Microtrac Bell). The measurement was performed after the spherical silica particles were dispersed by irradiating them with ultrasonic waves for 60 seconds three times in the device. The measurement was performed twice for 60 seconds each, and the average value was calculated.
  • MT3300EXII laser diffraction type particle size distribution analyzer
  • Viscosity of the kneaded product 6 parts by mass of boiled linseed oil (manufactured by Yamakei Sangyo Co., Ltd.) and 8 parts by mass of spherical silica particles were mixed, and the mixture was mixed at 2000 rpm using a rotation-revolution stirrer, Awatori Rentaro (manufactured by Shinky Co., Ltd.). The mixture was kneaded for 3 minutes to prepare a kneaded product. The obtained kneaded product was measured using a rotary rheometer at a shear rate of 1 s ⁇ 1 for 30 seconds, and the viscosity at 30 seconds was determined. The viscosity measured using boiled linseed oil alone was 46 mPa ⁇ s.
  • Viscosity of Silica Particle Dispersion 42 g of spherical silica particles and 18 g of methyl ethyl ketone (MEK) were placed in a 100 ml polybottle (solid content concentration 70% by mass), and stirred at 30 rpm for 2 hours using a mix rotor. The obtained mixed liquid was spouted three times at a pressure of 50 MPa from a ⁇ 0.1 mm nozzle using a wet atomization device (Starburst Mini manufactured by Sugino Machine Co., Ltd., model number: HJP-25001). repeated.
  • MEK methyl ethyl ketone
  • the resulting slurry was adjusted to 25°C, and its viscosity was measured using a rotary rheometer (Modular Rheometer PhysicaMCR-301, manufactured by Anton Paar) at a shear rate of 1 rpm for 30 seconds. The viscosity at that point was determined.
  • a rotary rheometer Modular Rheometer PhysicaMCR-301, manufactured by Anton Paar
  • PET5011 550 manufactured by Lintec Corporation, thickness 50 ⁇ m
  • the resulting varnish was applied to the release-treated surface of this PET film using an applicator so that the thickness after drying would be 40 ⁇ m, dried in a gear oven at 100°C for 10 minutes, and then cut lengthwise.
  • An uncured laminated film including an uncured resin film (B stage film) measuring 200 mm x width 200 mm x thickness 40 ⁇ m was produced. The obtained uncured laminated film was heated in a gear oven set at 190° C. for 90 minutes to harden the uncured resin film, thereby producing a cured film.
  • the lamination conditions were that the pressure was reduced to 13 hPa or less by reducing the pressure for 30 seconds, and then pressing was performed for 30 seconds at 100° C. and a pressure of 0.8 MPa.
  • Film peeling step The PET film of the laminated structure was peeled off.
  • Curing process The laminate was placed in a gear oven with an internal temperature of 180° C. for 30 minutes to cure the B-stage film and form an insulating layer.
  • evaluation sample B a strip-shaped cut with a width of 1 cm was made on the copper foil side.
  • the substrate was set in a 90° peel tester, the cut edge of the copper plating was picked up with a grip, 20 mm of the copper plating was peeled off, and the peel strength (N/cm) was measured.
  • Examples 1 to 7 had higher peel strength and stronger adhesive strength than Examples 8 to 10. Furthermore, in Examples 1 to 7, the graininess of the coating film was good, and all of them were suitable for practical use. On the other hand, in Examples 8 to 10, the peel strength was low and graininess of the coating film was also observed.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Wood Science & Technology (AREA)
  • Dispersion Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Silicon Compounds (AREA)
PCT/JP2023/016364 2022-05-09 2023-04-25 シリカ粒子分散液 Ceased WO2023218949A1 (ja)

Priority Applications (4)

Application Number Priority Date Filing Date Title
CN202380038964.2A CN119156348A (zh) 2022-05-09 2023-04-25 二氧化硅颗粒分散液
KR1020247036876A KR20250008054A (ko) 2022-05-09 2023-04-25 실리카 입자 분산액
JP2024520371A JPWO2023218949A1 (cg-RX-API-DMAC7.html) 2022-05-09 2023-04-25
US18/938,403 US20250059355A1 (en) 2022-05-09 2024-11-06 Silica particle dispersion liquid

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-077093 2022-05-09
JP2022077093 2022-05-09

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US18/938,403 Continuation US20250059355A1 (en) 2022-05-09 2024-11-06 Silica particle dispersion liquid

Publications (1)

Publication Number Publication Date
WO2023218949A1 true WO2023218949A1 (ja) 2023-11-16

Family

ID=88730319

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/016364 Ceased WO2023218949A1 (ja) 2022-05-09 2023-04-25 シリカ粒子分散液

Country Status (6)

Country Link
US (1) US20250059355A1 (cg-RX-API-DMAC7.html)
JP (1) JPWO2023218949A1 (cg-RX-API-DMAC7.html)
KR (1) KR20250008054A (cg-RX-API-DMAC7.html)
CN (1) CN119156348A (cg-RX-API-DMAC7.html)
TW (1) TW202400515A (cg-RX-API-DMAC7.html)
WO (1) WO2023218949A1 (cg-RX-API-DMAC7.html)

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2015036357A (ja) * 2013-08-13 2015-02-23 電気化学工業株式会社 表面処理シリカ粉末、スラリー組成物及びそれを用いた樹脂組成物
JP2019183005A (ja) * 2018-04-11 2019-10-24 Agc株式会社 フッ素樹脂シート、積層体及びそれらの製造方法

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP6348276B2 (ja) 2013-11-25 2018-06-27 日揮触媒化成株式会社 反射防止膜形成用塗布液および反射防止膜付基材とその製造方法ならびにその用途
JP6895760B2 (ja) 2017-02-03 2021-06-30 日揮触媒化成株式会社 シリカ系粒子分散液の製造方法、シリカ系粒子分散液、透明被膜形成用塗布液及び透明被膜付基材
JP6564517B1 (ja) 2018-12-17 2019-08-21 株式会社アドマテックス 電子材料用フィラー及びその製造方法、電子材料用樹脂組成物の製造方法、高周波用基板、並びに電子材料用スラリー

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2015036357A (ja) * 2013-08-13 2015-02-23 電気化学工業株式会社 表面処理シリカ粉末、スラリー組成物及びそれを用いた樹脂組成物
JP2019183005A (ja) * 2018-04-11 2019-10-24 Agc株式会社 フッ素樹脂シート、積層体及びそれらの製造方法

Also Published As

Publication number Publication date
KR20250008054A (ko) 2025-01-14
JPWO2023218949A1 (cg-RX-API-DMAC7.html) 2023-11-16
TW202400515A (zh) 2024-01-01
CN119156348A (zh) 2024-12-17
US20250059355A1 (en) 2025-02-20

Similar Documents

Publication Publication Date Title
WO2023008290A1 (ja) 球状シリカ粉末及び球状シリカ粉末の製造方法
WO2023218948A1 (ja) シリカ粒子分散液
WO2023100676A1 (ja) 中空シリカ粒子及びその製造方法
US20250100890A1 (en) Method for producing spherical silica powder
CN115667377A (zh) 分散液的制造方法
CN1910122A (zh) 无机粉末、用该粉末填充的树脂组合物及其用途
JP2022163625A (ja) 改質分散液の製造方法及び分散液
KR20250008054A (ko) 실리카 입자 분산액
JP2025152041A (ja) 窒化ホウ素粉末、及び、窒化ホウ素粉末の製造方法
JP7208842B2 (ja) 易解砕性銅粉及びその製造方法
WO2025182883A1 (ja) 球状シリカ粒子粉体及び球状シリカ粒子粉体の製造方法
WO2025182878A1 (ja) 球状シリカ粒子粉体及び球状シリカ粒子粉体の製造方法
WO2025182884A1 (ja) 球状シリカ粒子粉体及び球状シリカ粒子粉体の製造方法
WO2024237111A1 (ja) 球状シリカ粉末および球状シリカ粉末の製造方法
JP7806458B2 (ja) 改質粉体の製造方法
JP7708106B2 (ja) 分散液、複合粒子及び複合粒子の製造方法
JP2023181991A (ja) 球状シリカ粉末の製造方法
JP2023181992A (ja) 球状シリカ粉末の製造方法
JP2023181993A (ja) 球状シリカ粉末の製造方法
WO2025070232A1 (ja) 樹脂組成物およびシートモールディングコンパウンド、ならび樹脂組成物に使用されるアルミナ粒子
JP2023156243A (ja) 液状組成物、プリプレグ、樹脂付き金属基材、配線板及びシリカ粒子
CN117881736A (zh) 组合物、组合物的制造方法和片的制造方法
JP2024146810A (ja) 中空粒子を含む粉体、及びその製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23803429

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2024520371

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 202380038964.2

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 23803429

Country of ref document: EP

Kind code of ref document: A1