WO2023162605A1 - 非水系二次電池接着層用組成物、非水系二次電池用接着層、非水系二次電池用電池部材及びその製造方法、非水系二次電池用積層体及びその製造方法、並びに、非水系二次電池 - Google Patents
非水系二次電池接着層用組成物、非水系二次電池用接着層、非水系二次電池用電池部材及びその製造方法、非水系二次電池用積層体及びその製造方法、並びに、非水系二次電池 Download PDFInfo
- Publication number
- WO2023162605A1 WO2023162605A1 PCT/JP2023/003271 JP2023003271W WO2023162605A1 WO 2023162605 A1 WO2023162605 A1 WO 2023162605A1 JP 2023003271 W JP2023003271 W JP 2023003271W WO 2023162605 A1 WO2023162605 A1 WO 2023162605A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- secondary battery
- aqueous secondary
- adhesive layer
- polymer
- mass
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/409—Separators, membranes or diaphragms characterised by the material
- H01M50/411—Organic material
- H01M50/414—Synthetic resins, e.g. thermoplastics or thermosetting resins
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
- C09J133/00—Adhesives based on homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Adhesives based on derivatives of such polymers
- C09J133/04—Homopolymers or copolymers of esters
- C09J133/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, the oxygen atom being present only as part of the carboxyl radical
- C09J133/062—Copolymers with monomers not covered by C09J133/06
- C09J133/064—Copolymers with monomers not covered by C09J133/06 containing anhydride, COOH or COOM groups, with M being metal or onium-cation
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
- C09J11/00—Features of adhesives not provided for in group C09J9/00, e.g. additives
- C09J11/08—Macromolecular additives
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
- C09J5/00—Adhesive processes in general; Adhesive processes not provided for elsewhere, e.g. relating to primers
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M10/00—Secondary cells; Manufacture thereof
- H01M10/05—Accumulators with non-aqueous electrolyte
- H01M10/052—Li-accumulators
- H01M10/0525—Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M10/00—Secondary cells; Manufacture thereof
- H01M10/05—Accumulators with non-aqueous electrolyte
- H01M10/058—Construction or manufacture
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M10/00—Secondary cells; Manufacture thereof
- H01M10/05—Accumulators with non-aqueous electrolyte
- H01M10/058—Construction or manufacture
- H01M10/0583—Construction or manufacture of accumulators with folded construction elements except wound ones, i.e. folded positive or negative electrodes or separators, e.g. with "Z"-shaped electrodes or separators
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M10/00—Secondary cells; Manufacture thereof
- H01M10/42—Methods or arrangements for servicing or maintenance of secondary cells or secondary half-cells
- H01M10/4235—Safety or regulating additives or arrangements in electrodes, separators or electrolyte
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M4/00—Electrodes
- H01M4/02—Electrodes composed of, or comprising, active material
- H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M4/00—Electrodes
- H01M4/02—Electrodes composed of, or comprising, active material
- H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
- H01M4/139—Processes of manufacture
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M4/00—Electrodes
- H01M4/02—Electrodes composed of, or comprising, active material
- H01M4/62—Selection of inactive substances as ingredients for active masses, e.g. binders, fillers
- H01M4/621—Binders
- H01M4/622—Binders being polymers
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/403—Manufacturing processes of separators, membranes or diaphragms
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/409—Separators, membranes or diaphragms characterised by the material
- H01M50/411—Organic material
- H01M50/414—Synthetic resins, e.g. thermoplastics or thermosetting resins
- H01M50/42—Acrylic resins
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/409—Separators, membranes or diaphragms characterised by the material
- H01M50/443—Particulate material
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/409—Separators, membranes or diaphragms characterised by the material
- H01M50/449—Separators, membranes or diaphragms characterised by the material having a layered structure
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- H01M50/00—Constructional details or processes of manufacture of the non-active parts of electrochemical cells other than fuel cells, e.g. hybrid cells
- H01M50/40—Separators; Membranes; Diaphragms; Spacing elements inside cells
- H01M50/46—Separators, membranes or diaphragms characterised by their combination with electrodes
- H01M50/461—Separators, membranes or diaphragms characterised by their combination with electrodes with adhesive layers between electrodes and separators
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
- Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y02E60/00—Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
- Y02E60/10—Energy storage using batteries
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
- Y02P—CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS
- Y02P70/00—Climate change mitigation technologies in the production process for final industrial or consumer products
- Y02P70/50—Manufacturing or production processes characterised by the final manufactured product
Definitions
- the present invention provides a composition for a non-aqueous secondary battery adhesive layer, an adhesive layer for a non-aqueous secondary battery, a battery member for a non-aqueous secondary battery and a method for producing the same, a laminate for a non-aqueous secondary battery and a method for producing the same, It also relates to non-aqueous secondary batteries.
- Non-aqueous secondary batteries such as lithium-ion secondary batteries (hereinafter also referred to as “secondary batteries”) are small, lightweight, have high energy density, and have the characteristics of being capable of repeated charging and discharging (hereinafter referred to as “cycle characteristics”). ) and is used in a wide range of applications.
- a secondary battery generally includes a positive electrode, a negative electrode, and a battery member for a non-aqueous secondary battery such as a separator that separates the positive electrode and the negative electrode to prevent a short circuit between the positive electrode and the negative electrode (hereinafter referred to as "battery member ) is provided.
- a secondary battery uses a battery member provided with an adhesive layer to improve adhesion between battery members.
- the adhesive layer is usually formed by using a slurry-like non-aqueous secondary battery adhesive layer composition (hereinafter also referred to as "adhesive layer composition") containing a binder component and a solvent such as water. It is formed by supplying it onto a base material such as an electrode base material or a separator base material and drying it.
- Patent Literature 1 describes applying a non-aqueous secondary battery slurry containing a predetermined particulate polymer, a predetermined amount of a polyhydric alcohol compound, and water by an inkjet method. Further, in Patent Document 1, by using the non-aqueous secondary battery slurry, even when an inkjet method is adopted, strong adhesion between battery members and excellent low-temperature output characteristics of the secondary battery can be achieved. It has been reported that the adhesive material can be efficiently applied to the surface of the battery member while ensuring the adhesion.
- the adhesive layer composition of the prior art can be satisfactorily coated on a battery member by an inkjet method and can impart excellent adhesiveness to the battery members of a secondary battery, There is still room for improvement in terms of imparting excellent cycle characteristics to secondary batteries.
- the secondary battery is also required to have excellent electrolyte pourability (hereinafter also referred to as “electrolyte pourability”).
- the present invention provides a non-aqueous secondary battery with excellent electrolyte pourability while ensuring inkjet ejection characteristics, provides a non-aqueous secondary battery with excellent adhesiveness between battery members, and
- An object of the present invention is to provide a composition for a non-aqueous secondary battery adhesive layer capable of exhibiting excellent cycle characteristics in a non-aqueous secondary battery.
- the present invention imparts excellent electrolyte pourability to non-aqueous secondary batteries, imparts excellent adhesion between battery members to non-aqueous secondary batteries, and is excellent in non-aqueous secondary batteries.
- An object of the present invention is to provide an adhesive layer for a non-aqueous secondary battery, a battery member for a non-aqueous secondary battery, and a laminate for a non-aqueous secondary battery, which can exhibit excellent cycle characteristics.
- Another object of the present invention is to provide a non-aqueous secondary battery that is excellent in electrolyte pourability, adhesion between battery members, and cycle characteristics.
- the present invention imparts excellent electrolyte pourability to non-aqueous secondary batteries, imparts excellent adhesion between battery members to non-aqueous secondary batteries, and is excellent in non-aqueous secondary batteries.
- An object of the present invention is to provide a method for manufacturing a battery member for a non-aqueous secondary battery and a method for manufacturing a laminate for a non-aqueous secondary battery, which can exhibit excellent cycle characteristics.
- the inventor of the present invention conducted intensive studies with the aim of solving the above problems. Then, the present inventors have found that a particulate polymer, a predetermined polyalkylene glycol, and water are included, and the content of the polyalkylene glycol per 100 parts by mass of the particulate polymer is a predetermined numerical value or more. The inventors have found that the above problems can be solved by a composition for a non-aqueous secondary battery adhesive layer, and have completed the present invention.
- an object of the present invention is to advantageously solve the above problems, and the present invention provides a non-aqueous secondary battery adhesive layer containing a particulate polymer, polyalkylene glycol, and water.
- the composition wherein the polyalkylene glycol comprises ethylene oxide units, propylene oxide units, or a combination thereof, the polyalkylene glycol having one end group that is a hydroxy group and the other end group that is a hydroxy group.
- the number average molecular weight of the polyalkylene glycol is 150 to 1200, and the content of the polyalkylene glycol is 100 mass of the particulate polymer
- It is a composition for a non-aqueous secondary battery adhesive layer which is 20 parts by mass or more per part. With such a composition for a non-aqueous secondary battery adhesive layer, while ensuring inkjet ejection characteristics, it imparts excellent electrolyte pourability to a non-aqueous secondary battery, and a battery member for a non-aqueous secondary battery. It is possible to impart excellent adhesion between them and to exhibit excellent cycle characteristics in the non-aqueous secondary battery.
- "number average molecular weight" can be measured using the method described in the Examples of the present specification.
- the particulate polymer has a core-shell structure comprising a core and a shell covering at least a portion of the outer surface of the core. It is preferably coalesced. If the particulate polymer is a particulate polymer having a core-shell structure, the core portion and the shell portion can exhibit different functions, and the inkjet ejection characteristics can be improved.
- the particulate polymer preferably contains a polymer having a glass transition temperature of 40° C. or higher. If the particulate polymer contains a polymer having a glass transition temperature of 40° C. or higher, the inkjet ejection characteristics can be improved.
- the "glass transition temperature” can be measured using the measurement method described in the Examples of the specification.
- the composition for a non-aqueous secondary battery adhesive layer of the present invention further contains a water-soluble polymer as a dispersant. If the non-aqueous secondary battery adhesive layer composition further contains a water-soluble polymer as a dispersant, the inkjet discharge characteristics, the adhesion between the electrode members of the non-aqueous secondary battery, and the electrolyte injection of the non-aqueous secondary battery and the cycle characteristics of the non-aqueous secondary battery can be improved.
- Another object of the present invention is to advantageously solve the above-mentioned problems. is.
- Such an adhesive layer for a non-aqueous secondary battery imparts excellent electrolyte pourability to the non-aqueous secondary battery, imparts excellent adhesion between battery members to the non-aqueous secondary battery, In addition, the non-aqueous secondary battery can exhibit excellent cycle characteristics.
- Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention comprises a base material and the non-aqueous secondary battery adhesive layer provided on the base material. and a battery member for a non-aqueous secondary battery, wherein the substrate is an electrode substrate or a separator.
- a battery member for a non-aqueous secondary battery imparts excellent electrolyte pourability to the non-aqueous secondary battery, imparts excellent adhesiveness between the battery members to the non-aqueous secondary battery,
- the non-aqueous secondary battery can exhibit excellent cycle characteristics.
- Another object of the present invention is to advantageously solve the above-mentioned problems. and drying the non-aqueous secondary battery adhesive layer composition coated on the electrode base material or the separator base material, a battery member for a non-aqueous secondary battery, is a manufacturing method.
- a method for manufacturing a battery member for a non-aqueous secondary battery excellent electrolyte pourability is imparted to the non-aqueous secondary battery, and excellent adhesiveness between battery members is imparted to the non-aqueous secondary battery. It is possible to obtain a battery member for a non-aqueous secondary battery that can impart excellent cycle characteristics to the non-aqueous secondary battery.
- the base material is an electrode base material
- the non-aqueous secondary battery adhesive layer composition is applied onto the electrode mixture layer of the electrode base material. It is preferable to work
- a battery member for a non-aqueous secondary battery capable of exhibiting superior cycle characteristics to a non-aqueous secondary battery is obtained by coating the composition for a non-aqueous secondary battery adhesive layer on the electrode mixture layer of the electrode base material. be able to.
- Another object of the present invention is to advantageously solve the above problems, and the present invention provides a laminate for a non-aqueous secondary battery comprising an electrode and a separator, is a laminate for a non-aqueous secondary battery bonded via the adhesive layer for a non-aqueous secondary battery.
- a laminate for a non-aqueous secondary battery imparts excellent electrolyte pourability to the non-aqueous secondary battery, imparts excellent adhesiveness between battery members to the non-aqueous secondary battery,
- the non-aqueous secondary battery can exhibit excellent cycle characteristics.
- Another object of the present invention is to advantageously solve the above-mentioned problems. and a step of pressing and bonding the electrode and the separator through the bonded surface, wherein the adhesive material is a non-aqueous secondary battery adhesive layer composition using the non-aqueous secondary battery adhesive layer composition.
- This is a method for manufacturing a laminate for a secondary battery. With such a method for producing a laminate for a non-aqueous secondary battery, excellent electrolyte pourability is imparted to the non-aqueous secondary battery, and excellent adhesiveness between battery members is imparted to the non-aqueous secondary battery. It is possible to obtain a laminate for a non-aqueous secondary battery that can impart excellent cycle characteristics to the non-aqueous secondary battery.
- Another object of the present invention is to advantageously solve the above problems, and the present invention is a non-aqueous secondary battery comprising the above-described non-aqueous secondary battery laminate.
- a non-aqueous secondary battery is excellent in electrolyte pourability, adhesion between battery members, and cycle characteristics.
- the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesion between battery members, and It is possible to provide a non-aqueous secondary battery adhesive layer composition capable of exhibiting excellent cycle characteristics in a non-aqueous secondary battery. Further, according to the present invention, the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesiveness between battery members, and the non-aqueous secondary battery It is possible to provide an adhesive layer for a non-aqueous secondary battery, a battery member for a non-aqueous secondary battery, and a laminate for a non-aqueous secondary battery that can exhibit excellent cycle characteristics.
- non-aqueous secondary battery that is excellent in electrolyte pourability, adhesion between battery members, and cycle characteristics. Further, according to the present invention, the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesiveness between battery members, and the non-aqueous secondary battery It is possible to provide a method for manufacturing a battery member for a non-aqueous secondary battery and a method for manufacturing a laminate for a non-aqueous secondary battery, which can exhibit excellent cycle characteristics.
- FIG. 1 is a cross-sectional view schematically showing the structure of an example of a particulate polymer having a core-shell structure;
- FIG. It is a figure explaining an example of the manufacturing process of the laminated body for non-aqueous secondary batteries of this invention. It is a figure explaining the manufacturing process of the laminated body for non-aqueous secondary batteries in an Example and a comparative example.
- the composition for non-aqueous secondary battery adhesive layer of the present invention can be used when forming the adhesive layer for non-aqueous secondary battery of the present invention (hereinafter also referred to as "adhesive layer”).
- the non-aqueous secondary battery adhesive layer composition of the present invention is used as the battery member for non-aqueous secondary batteries of the present invention and the laminate for non-aqueous secondary batteries of the present invention (hereinafter also referred to as "laminate").
- the battery member for a non-aqueous secondary battery and the laminate for a non-aqueous secondary battery of the present invention can be used when producing the non-aqueous secondary battery of the present invention. It can be manufactured by a method for manufacturing a battery member for a non-aqueous secondary battery and a method for manufacturing a laminate for a non-aqueous secondary battery.
- the non-aqueous secondary battery adhesive layer composition of the present invention contains a particulate polymer, a predetermined polyalkylene glycol to be described later, and water, and may optionally contain other components.
- Other components include, for example, binders, low-molecular-weight polyhydric alcohol compounds, dispersants, thixotropic agents, and solvents other than water.
- the adhesive layer composition is a slurry composition in which a particulate polymer is dispersed in water.
- the particulate polymer contained in the adhesive layer composition of the present invention is hydrophobic because it is dispersed in water.
- the polyalkylene glycol contained in the composition for an adhesive layer of the present invention is a linear molecule, and includes an ethylene oxide unit ( --CH.sub.2CH.sub.2O-- ), a propylene oxide unit ( --CHCH.sub.3CH.sub.2O-- or --CH 2 CHCH 3 O—), or a unit combining these.
- one terminal group hereinafter also referred to as "terminal group A”
- the other terminal group hereinafter also referred to as "terminal group B”
- terminal group B is a hydroxy group or It is an alkoxy group having 1 to 6 carbon atoms and a number average molecular weight of 150 to 1,200.
- the content of polyalkylene glycol per 100 parts by mass of the particulate polymer is 20 parts by mass or more.
- the adhesive layer composition provides excellent electrolyte pourability to non-aqueous secondary batteries while ensuring inkjet ejection characteristics, and provides non-aqueous secondary batteries with excellent adhesiveness between battery members.
- the non-aqueous secondary battery can exhibit excellent cycle characteristics. It is presumed that these are due to the mutual combination of moisturizing function, dispersion stabilizing function, thickening effect, surface activity, etc. possessed by the polyalkylene glycol, but the reason is not necessarily clear. is not.
- the terminal group A is a hydroxy group
- the terminal group B is a hydroxy group or has one carbon atom, including ethylene oxide units, propylene oxide units, or units in which these are combined.
- the adhesive layer composition is , while ensuring inkjet ejection characteristics, imparting excellent electrolyte pourability to the secondary battery, imparting excellent adhesion between battery members to the secondary battery, and excellent cycle characteristics to the secondary battery
- polyalkylene glycols in which the terminal group B is an alkoxy group having 1 to 6 carbon atoms include triethylene glycol monobutyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and the like.
- the terminal group B of the polyalkylene glycol is preferably a hydroxy group because it can improve the adhesion between battery members of the secondary battery and improve the cycle characteristics of the secondary battery.
- the arrangement order of the ethylene oxide units and propylene oxide units may be alternating, random or block.
- the sequence of ethylene oxide units and propylene oxide units is preferably block.
- the ratio of ethylene oxide units to propylene oxide units (ethylene oxide units/propylene oxide units) in terms of moles is, for example, 1/20 or more, and 1/ It may be 10 or more, for example, 20/1 or less, 10/1 or less, 1/1 or less, or 1/3 or less.
- the total content of ethylene oxide units and propylene oxide units in the polyalkylene glycol is preferably 70 mol% or more, preferably 80 mol% or more, based on 100 mol% of all repeating units contained in the polyalkylene glycol. is more preferably 90 mol % or more, and particularly preferably 100 mol %, that is, the polyalkylene glycol consists only of ethylene oxide units and/or propylene oxide units.
- polyalkylene glycol consisting only of ethylene oxide units is also referred to as "polyethylene glycol”
- polyalkylene glycol consisting only of propylene oxide units is also referred to as “polypropylene glycol”
- polyalkylene glycol consisting only of ethylene oxide units and propylene oxide units is also referred to as “polypropylene glycol”.
- polyoxyethylene polyoxypropylene glycol is also referred to as "polyoxyethylene polyoxypropylene glycol”.
- polyethylene glycol or polypropylene glycol is preferable, and polyethylene glycol is more preferable, because it can improve the inkjet ejection characteristics, the electrolyte pourability of the secondary battery, and the cycle characteristics of the secondary battery.
- the ratio of various monomer units in polyalkylene glycols and polymers can be measured using nuclear magnetic resonance (NMR) methods such as 1 H-NMR and 13 C-NMR.
- the polyalkylene glycol may contain monomeric units other than ethylene oxide units and propylene oxide units.
- Other monomeric units include, for example, butylene oxide units, octene oxide units, and the like.
- the content of other monomer units in the polyalkylene glycol is It is preferably 30 mol% or less, more preferably 20 mol% or less, still more preferably 10 mol% or less, based on 100 mol% of the total repeating units containing , it is particularly preferred that the polyalkylene glycol does not contain other monomeric units.
- the number average molecular weight of the polyalkylene glycol is preferably 300 or more, more preferably 400 or more, still more preferably 500 or more, preferably 1050 or less, and preferably 900 or less. It is more preferably 700 or less, and even more preferably 600 or less.
- the cycle characteristics of the secondary battery can be further improved.
- the number average molecular weight of the polyalkylene glycol is equal to or less than the above upper limit, the inkjet ejection characteristics can be improved. Further, when the number average molecular weight of the polyalkylene glycol is within the above range, the adhesiveness between the electrode members of the secondary battery can be improved.
- the content of the polyalkylene glycol should be 20 parts by mass or more, preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and 60 parts by mass per 100 parts by mass of the particulate polymer. More preferably, it is at least 1 part.
- the content of the polyalkylene glycol is at least the above lower limit, it is possible to improve inkjet discharge characteristics, adhesiveness between electrode members of a secondary battery, electrolyte pourability of a secondary battery, and cycle characteristics of a secondary battery.
- the content of the polyalkylene glycol is, for example, 150 parts by mass or less per 100 parts by mass of the particulate polymer, and may be 100 parts by mass or less.
- the content of polyalkylene glycol in the adhesive layer composition is preferably 20% by mass or less, and 10% by mass or less, relative to the entire adhesive layer composition (including solvents such as water, which will be described later). More preferably, it is 5% by mass or less.
- the content of polyalkylene glycol in the adhesive layer composition is equal to or less than the above upper limit, it is possible to improve ink-jet ejection characteristics and adhesiveness between electrode members of a secondary battery.
- the content of the polyalkylene glycol in the adhesive layer composition is, for example, 0.1% by mass or more and 0.5% by mass or more with respect to the entire adhesive layer composition.
- the particulate polymer contained in the adhesive layer composition of the present invention is a component that functions as an adhesive material in the adhesive layer that bonds battery members such as separators and electrodes.
- the adhesive layer composition may contain only one type of particulate polymer, or may contain two or more types of particulate polymers.
- the content of the particulate polymer in the adhesive layer composition is preferably 1% by mass or more, preferably 3% by mass, based on the entire adhesive layer composition (including a solvent such as water, which will be described later). It is more preferably 15% by mass or less, and more preferably 10% by mass or less. If the content of the particulate polymer is at least the above lower limit, the adhesion between the electrode members of the secondary battery can be improved. On the other hand, when the content of the particulate polymer is equal to or less than the above upper limit, the inkjet ejection characteristics can be improved.
- the particulate polymer preferably contains a polymer having a glass transition temperature of 40°C or higher. If the particulate polymer contains a polymer having a glass transition temperature of 40° C. or higher, the inkjet ejection characteristics can be improved. At least part of the surface of the particulate polymer is preferably composed of a polymer having a glass transition temperature of 40° C. or higher.
- the glass transition temperature of the polymer that can be contained in the particulate polymer is preferably 50° C. or higher, more preferably 80° C. or higher, preferably 200° C. or lower, and 120° C. The following are more preferable.
- the inkjet ejection characteristics can be further improved.
- the glass transition temperature of the polymer is equal to or lower than the above upper limit, so that an adhesive layer can be formed that more strongly bonds the battery members together even when pressurized at room temperature.
- the glass transition temperature of the polymer can be adjusted, for example, by changing the types and proportions of monomers used in preparing the polymer.
- the particulate polymer preferably has a water contact angle of 10° or more, more preferably 15° or more, preferably 90° or less, and more preferably 80° or less. If the water contact angle is within the above range, the particulate polymer can have good hydrophobicity, and as a result, the dispersibility of the particulate polymer in the adhesive layer composition can be improved. It can also interact well with polyalkylene glycols.
- the "water contact angle" is obtained by coating an aqueous dispersion of the particulate polymer on the separator base material, and 2 microliters of ion-exchanged water is dropped on the surface of the layer composed of the particulate polymer.
- the contact angle meter manufactured by Kyowa Interface Science Co., Ltd., "PCA-1" can be used to measure the droplet after 1 second.
- the volume average particle diameter of the particulate polymer is preferably 100 nm or more, more preferably 200 nm or more, still more preferably 400 nm or more, even more preferably 500 nm or more, and 1500 nm or less. is preferably 900 nm or less, more preferably 800 nm or less, and even more preferably 700 nm or less.
- the volume-average particle size of the particulate polymer is at least the above lower limit, it is possible to suppress deterioration of battery characteristics due to an increase in resistance of the secondary battery due to hindrance to the path of lithium ions in the substrate (electrode or separator).
- volume average particle size refers to the particle size at which the cumulative volume calculated from the small size side is 50% in the volume-based particle size distribution measured by laser diffraction. It can be measured using the measuring method described in the Examples.
- the particulate polymer may be particles composed of a single polymer, or particles composed of a composite of a plurality of polymers (two or more polymers are physically or chemically bonded). It may be a particle formed by Among them, from the viewpoint of being able to exhibit multiple properties, the particulate polymer is preferably particles in which a plurality of polymers are combined, and the core portion and the shell portion covering at least a part of the outer surface of the core portion.
- particles with a core-shell structure particles with a side-by-side structure in which two or more polymers are arranged side by side; particles with a snowball structure in which a part of the central polymer is exposed to the outer shell; Particles having a octopus structure, which is a structure in which polymer particles of a different kind are embedded in the surface of the polymer particles of No. 1, are more preferred, and particles having a core-shell structure are even more preferred.
- a particulate polymer having a core-shell structure will be described below as an example.
- a particulate polymer having a core-shell structure has a core-shell structure comprising a core portion and a shell portion covering the outer surface of the core portion. Inkjet ejection characteristics can be improved by using a particulate polymer having a core-shell structure.
- the shell portion may cover the entire outer surface of the core portion, or may partially cover the outer surface of the core portion. Even if the outer surface of the core portion appears to be completely covered by the shell portion, if a hole is formed to allow communication between the inside and outside of the shell portion, the shell portion can be replaced by the core portion. is a shell part that partially covers the outer surface of the
- particulate polymer 300 has a core-shell structure with core portion 310 and shell portion 320 .
- the core portion 310 is a portion inside the shell portion 320 in the particulate polymer 300 .
- the shell part 320 is a part that covers the outer surface 310S of the core part 310 and is usually the outermost part of the particulate polymer 300 .
- the shell portion 320 does not cover the entire outer surface 310S of the core portion 310 but partially covers the outer surface 310S of the core portion 310 .
- the particulate polymer may have any constituent elements other than the above-described core portion and shell portion as long as they do not significantly impair the desired effect.
- the particulate polymer may have a portion formed of a polymer different from the core portion inside the core portion.
- the seed particles used in the production of the particulate polymer by the seed polymerization method may remain inside the core portion.
- the particulate polymer has only the core portion and the shell portion.
- the glass transition temperature of the polymer of the core portion of the particulate polymer is preferably ⁇ 50° C. or higher, more preferably ⁇ 45° C. or higher, preferably 60° C. or lower, and 35° C. or lower. It is more preferably 0° C. or lower, and even more preferably ⁇ 15° C. or lower.
- the glass transition temperature of the core polymer is equal to or higher than the above lower limit, the inkjet ejection characteristics can be improved.
- the core polymer can exhibit good adhesiveness, and as a result, the battery members can be more strongly bonded together even when pressurized at room temperature. An adhesive layer that adheres can be formed.
- the glass transition temperature of the polymer of the core portion is equal to or lower than the above upper limit, it is possible to sufficiently prevent the components contained in the adhesive layer from coming off (so-called falling powder).
- the glass transition temperature of the core polymer can be adjusted, for example, by changing the types and proportions of the monomers used in the preparation of the core polymer.
- monomers used for preparing the core polymer include vinyl chloride-based monomers such as vinyl chloride and vinylidene chloride; vinyl acetate-based monomers such as vinyl acetate; styrene and ⁇ -methylstyrene.
- styrenesulfonic acid butoxystyrene, vinylnaphthalene and other aromatic vinyl monomers
- vinylamine-based monomers such as vinylamine
- N-vinylformamide N-vinylacetamide and other vinylamide-based monomers
- methyl acrylate ethyl acrylate
- Fluorine-free (meth)acrylic acid ester monomers such as , n-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and cyclohexyl methacrylate
- (meth)acrylamide monomers such as acrylamide and methacrylamide monomers
- (meth)acrylonitrile monomers such as acrylonitrile and methacrylonitrile
- fluorine-containing (meth)acrylate monomers such as 2-(perfluorohexyl)ethyl methacrylate and 2-(per
- (meth)acryl means acryl and/or methacryl
- (meth)acrylonitrile means acrylonitrile and/or methacrylonitrile.
- fluorine-free (meth)acrylic acid ester monomer and “fluorine-containing (meth)acrylic acid ester monomer” are collectively referred to as “(meth)acrylic acid ester monomer”. .
- the monomer used for the preparation of the polymer of the core portion is at least a (meth)acrylic acid ester monomer from the viewpoint of further firmly bonding the battery members together via the adhesive layer. It is preferable to use a body, and a combination of a (meth) acrylic acid ester monomer and an aromatic vinyl monomer, or a combination of a (meth) acrylic acid ester monomer and a (meth) acrylonitrile monomer more preferred. That is, the polymer of the core portion preferably contains at least (meth) acrylic acid ester monomer units, and (meth) acrylic acid ester monomer units and aromatic vinyl monomer units or (meth) acrylonitrile It is more preferable to include a monomer unit.
- the (meth)acrylic acid ester monomer that can be used for preparing the core polymer is preferably a fluorine-free (meth)acrylic acid ester monomer. That is, the (meth)acrylic acid ester monomer units that can be contained in the core polymer are preferably fluorine-free (meth)acrylic acid ester monomer units.
- "containing a monomer unit” means "a repeating unit derived from the monomer is contained in the polymer obtained using the monomer”.
- the term "(meth)acrylic acid ester monomer” refers to a monofunctional (meth)acrylic acid ester monomer having only one polymerizable group.
- the ratio of the (meth)acrylic acid ester monomer unit in the polymer of the core part is the particulate polymer (consisting of only the core part and the shell part) from the viewpoint of further firmly bonding the battery members through the adhesive layer
- a particulate polymer it is preferably 5% by mass or more based on 100% by mass of all repeating units (total monomer units) in the core polymer and the shell polymer). It is more preferably 20% by mass or more, particularly preferably 20% by mass or more, preferably 98% by mass or less, and more preferably 96% by mass or less.
- the weight of the core is The ratio of the (meth)acrylic acid ester monomer unit in the coalescence is the particulate polymer (in the case of a particulate polymer consisting only of the core portion and the shell portion, the polymer of the core portion and the polymer of the shell portion).
- All repeating units (all monomer units) in the particulate polymer are 100 mass % is preferably 15% by mass or more, more preferably 20% by mass or more, particularly preferably 25% by mass or more, preferably 90% by mass or less, and 80% by mass or less. It is more preferable that the content is 70% by mass or less, and it is particularly preferable that the content is 70% by mass or less.
- the core portion contains (meth)acrylic acid ester monomer units and (meth)acrylonitrile monomer units, from the viewpoint of further firmly bonding the battery members together via the adhesive layer, the core portion
- the ratio of the (meth)acrylic acid ester monomer unit in the polymer is the particulate polymer (in the case of a particulate polymer consisting only of the core and shell, the weight of the core polymer and the shell It is preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 85% by mass or more, based on 100% by mass of all repeating units (total monomer units) in the coalescence).
- the proportion of (meth)acrylonitrile monomer units in the polymer of the core part is the particulate polymer (core part In the case of a particulate polymer consisting only of and a shell portion, the total repeating units (total monomer units) in the core polymer and the shell portion) are 100% by mass, and 1% by mass or more It is preferably 1.5% by mass or more, more preferably 10% by mass or less, and more preferably 5% by mass or less.
- the core polymer may contain an acid group-containing monomer unit.
- the acid group-containing monomer includes a monomer having an acid group, such as a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, and a monomer having a phosphoric acid group. be done.
- Examples of monomers having a carboxylic acid group include monocarboxylic acids and dicarboxylic acids.
- monocarboxylic acids include acrylic acid, methacrylic acid, crotonic acid and the like.
- dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid.
- monomers having a sulfonic acid group include vinylsulfonic acid, methylvinylsulfonic acid, (meth)allylsulfonic acid, ethyl (meth)acrylate-2-sulfonate, and 2-acrylamido-2-methyl propanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and the like.
- the monomer having a phosphate group includes, for example, 2-(meth)acryloyloxyethyl phosphate, methyl 2-(meth)acryloyloxyethyl phosphate, ethyl phosphate-(meth)acryloyloxyethyl etc.
- (meth)allyl means allyl and/or methallyl
- (meth)acryloyl means acryloyl and/or methacryloyl.
- the acid group-containing monomer a monomer having a carboxylic acid group is preferable, monocarboxylic acid is preferable, and (meth)acrylic acid is more preferable.
- one type of acid group-containing monomer may be used alone, or two or more types may be used in combination at an arbitrary ratio.
- the proportion of the acid group-containing unit in the core polymer is determined by the particulate polymer (in the case of a particulate polymer consisting only of the core and shell, the core polymer and the shell polymer). Based on 100% by mass of all repeating units (total monomer units) in the , 10% by mass or less.
- the proportion of the acid group-containing unit within the above range, the dispersibility of the polymer in the core portion is enhanced during preparation of the particulate polymer, and the outer surface of the core portion is greater than the outer surface of the polymer in the core portion. can be made easier to form a shell part that partially covers the .
- the polymer of the core portion preferably contains crosslinkable monomer units in addition to the above monomer units.
- a crosslinkable monomer is a monomer that can form a crosslinked structure during or after polymerization by heating or irradiation with energy rays.
- crosslinkable monomers include polyfunctional monomers having two or more polymerization reactive groups in the monomer.
- polyfunctional monomers include divinyl benzene, 1,3-butadiene, isoprene, divinyl monomers such as allyl methacrylate; ethylene dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, Di(meth)acrylic acid ester monomers such as 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester monomers such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; allyl glycidyl ether, glycidyl Ethylenically unsaturated monomers containing an epoxy group such as methacrylate; ⁇ -methacryloxypropyltrimethoxysilane, N-methylolacrylamide and the like.
- di(meth)acrylate monomers are examples of such as
- the ratio of the crosslinkable monomer units in the polymer of the core part is the particulate polymer (in the case of a particulate polymer consisting only of the core part and the shell part, the polymer of the core part and the polymer of the shell part). It is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and 10% by mass or less based on 100% by mass of all repeating units (total monomer units) in is preferred, 5% by mass or less is more preferred, and 3% by mass or less is particularly preferred.
- the proportion of the crosslinkable monomer unit within the above range, the battery members can be further strongly adhered to each other via the adhesive layer.
- the glass transition temperature of the polymer of the shell portion of the particulate polymer is preferably 40° C. or higher, more preferably 50° C. or higher, still more preferably 80° C. or higher, and 200° C. or lower. is preferred, and 120° C. or lower is more preferred.
- the glass transition temperature of the polymer of the shell portion is equal to or higher than the above lower limit, the inkjet ejection characteristics can be further improved.
- the glass transition temperature of the shell polymer is below the above upper limit, the particulate polymer will be moderately soft, forming an adhesive layer that more firmly bonds the battery members together even when pressurized at room temperature. can.
- the glass transition temperature of the shell polymer can be adjusted, for example, by changing the types and proportions of the monomers used in preparing the shell polymer.
- the glass transition temperature of the polymer of the shell part is the glass transition temperature of the polymer of the core part described above, from the viewpoint of maintaining the shape of the particulate polymer after adhesion between the battery members and suppressing an increase in resistance. is preferably 25° C. or more higher than.
- the monomer used for preparing the polymer for the shell portion examples include the same monomers as those exemplified as the monomers that can be used for producing the polymer for the core portion. Moreover, such a monomer may be used individually by 1 type, and may be used in combination of 2 or more types by arbitrary ratios.
- a (meth)acrylic acid ester monomer is used as the monomer used for preparing the polymer of the shell portion from the viewpoint of more firmly bonding the battery members together via the adhesive layer.
- aromatic vinyl monomers, (meth)acrylonitrile monomer units and acid group-containing monomers are more preferably used. That is, the polymer of the shell portion contains at least one of (meth)acrylic acid ester monomer units, aromatic vinyl monomer units, (meth)acrylonitrile monomer units and acid group-containing monomer units. is preferred.
- the ratio of the (meth)acrylic acid ester monomer unit in the polymer of the shell part is determined from the viewpoint of further firmly bonding the battery members together via the adhesive layer, so that the particulate polymer (the core part and the shell part In the case of a particulate polymer consisting of only, the total repeating units (total monomer units) in the core polymer and the shell polymer) is 100% by mass, and the content is 1% by mass or more. It is preferably 1.5% by mass or more, more preferably 10% by mass or less, and more preferably 6% by mass or less.
- the ratio of the aromatic vinyl monomer unit in the polymer of the shell part is determined from the viewpoint of more firmly bonding the battery members together via the adhesive layer.
- a polymer it is preferably 2% by mass or more, preferably 3% by mass, based on 100% by mass of all repeating units (total monomer units) in the core polymer and the shell polymer). It is more preferably 10% by mass or less, and more preferably 5% by mass or less.
- the ratio of the (meth)acrylonitrile monomer unit in the shell polymer is determined by the particulate polymer (in the case of a particulate polymer consisting of only the core and shell, the weight of the core polymer and the shell). Assuming that the total repeating units (total monomer units) in the coalescence is 100% by mass, the content is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and 2% by mass or less. It is preferably 1% by mass or less, more preferably 0.5% by mass or less.
- the ratio of the acid group-containing monomer in the polymer of the shell part is the particulate polymer (in the case of a particulate polymer consisting only of the core part and the shell part, the polymer of the core part and the polymer of the shell part). It is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and 1% by mass or less, based on 100% by mass of all repeating units (total monomer units) in is preferred, 0.5% by mass or less is more preferred, and 0.2% by mass or less is even more preferred.
- the mass ratio of the shell portion to the total of the core portion and the shell portion is preferably 2% by mass or more, preferably 20% by mass or less, and more preferably 15% by mass or less. It is preferably 10% by mass or less, and particularly preferably 5% by mass or less.
- the mass ratio of the shell portion is equal to or higher than the above lower limit, the inkjet ejection characteristics can be further improved.
- the mass ratio of the shell portion is equal to or less than the above upper limit, it is possible to form an adhesive layer that more firmly bonds the battery members together even with room temperature pressurization.
- the mass ratio of the shell portion to the total of the core portion and the shell portion is calculated from the thickness ratio of the core portion and the shell portion and the specific gravity of the particulate polymer, which will be described later.
- the ratio of the average shell thickness to the volume average particle diameter of the particulate polymer is preferably 0.1% or more, more preferably 0.5% or more, preferably 15% or less, and more preferably 10% or less. .
- the average thickness of the shell portion is at least the above lower limit, the inkjet ejection characteristics can be further improved.
- the battery members can be adhered to each other more firmly when the battery members are pressurized at room temperature.
- the average thickness of the shell portion of the particulate polymer is obtained by observing the cross-sectional structure of the particulate polymer using a transmission electron microscope (TEM). Specifically, the maximum thickness of the shell portion in the cross-sectional structure of the particulate polymer is measured using a TEM, and the average value of the maximum thickness of the shell portions of arbitrarily selected 20 or more particulate polymer particles is calculated. , the average thickness of the shell.
- the shell portion is composed of polymer particles, and the particles constituting the shell portion do not overlap in the radial direction of the particulate polymer particles, and the polymer particles are in a single layer. When the shell portion is formed, the number average particle diameter of the particles forming the shell portion is taken as the average thickness of the shell portion.
- the particulate polymer described above uses, for example, a monomer of the core polymer and a monomer of the shell polymer, and the ratio of these monomers is changed over time to form a can be prepared by direct polymerization.
- the particulate polymer can be prepared by sequential multistage emulsion and suspension polymerization processes in which earlier stage polymer is sequentially coated by later stage polymer. can.
- emulsifiers such as anionic surfactants such as sodium dodecylbenzenesulfonate and sodium dodecylsulfate, nonionic surfactants such as polyoxyethylene nonylphenyl ether and sorbitan monolaurate, or Cationic surfactants such as octadecylamine acetate can be used.
- peroxides such as t-butyl peroxy-2-ethylhexanoate, potassium persulfate, cumene peroxide, 2,2′-azobis(2-methyl-N-(2 -hydroxyethyl)-propionamide), 2,2'-azobis(2-amidinopropane) hydrochloride, and other azo compounds can be used.
- the monomers forming the core portion and the emulsifier are mixed, and emulsion polymerization is performed all at once to obtain a particulate polymer forming the core portion.
- the above particulate polymer can be obtained by polymerizing the monomer forming the shell in the presence of the particulate polymer composing the core.
- the monomers forming the polymer of the shell portion are divided into a plurality of times or continuously. It is preferable to supply to the polymerization system at the same time. By dividing or continuously supplying the monomer forming the shell polymer to the polymerization system, the polymer forming the shell is formed into particles, and the particles are bonded to the core. Thus, a shell portion that partially covers the core portion can be formed.
- the particulate polymer having a core-shell structure has been described above as an example, but the polymer of the core portion and the polymer of the shell portion mentioned above are the polymers constituting the particulate polymer having a structure other than the core-shell structure. May be used as a combination. That is, the particulate polymer composed of a single polymer may be composed of the polymer described above as the polymer of the core portion, or may be composed of the polymer described above as the polymer of the shell portion. .
- a particulate polymer having a structure other than a core-shell structure, which is formed by compositing a plurality of polymers is a composite of the polymer described above as the polymer for the core portion and the polymer described above as the polymer for the shell portion.
- the adhesive layer composition of the present invention contains water as a solvent, and may optionally contain a solvent other than water.
- solvents other than water include cyclic aliphatic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; ketones such as ethyl methyl ketone and cyclohexanone; -esters such as butyrolactone and ⁇ -caprolactone; nitriles such as acetonitrile and propionitrile; ethers such as tetrahydrofuran; and organic solvents such as alcohols such as methanol, ethanol and isopropanol.
- the adhesive layer composition of the present invention may contain a binder.
- the binder prevents components contained in the adhesive layer from falling off.
- the binder may consist of a polymer that dissolves in the solvent, or may consist of a polymer that does not dissolve in the solvent.
- the solvent-insoluble polymer may exist in the form of a particulate binder in the adhesive layer composition.
- the glass transition temperature of the polymer used as the binder is preferably 25° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower.
- the glass transition temperature of the polymer is 25° C. or lower, the components contained in the adhesive layer can be sufficiently prevented from coming off, and the adhesiveness between the battery members of the secondary battery can be improved.
- monomers used for preparing the polymer as the binder include (meth)acrylic acid ester monomers, (meth)acrylonitrile monomers, aromatic vinyl monomer units, acid group-containing monomers, monomers, (meth)acrylamide monomers, crosslinkable monomers, and the like can be used.
- the monomer used for preparing the polymer as the binder includes, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate and the like (meth)acryl having a polar group. Acid ester monomers can also be used.
- the said monomer may be used individually by 1 type, and may be used in combination of 2 or more types by arbitrary ratios.
- monomers used to prepare a polymer as a binder include (meth)acrylic acid ester monomers, (meth)acrylonitrile monomers, acid group-containing monomers, (meth) An acrylamide monomer and a crosslinkable monomer may be combined, or an aromatic vinyl monomer, an acid group-containing monomer, a (meth)acrylic acid ester monomer having a polar group, and a crosslinkable monomer.
- the polymer as a binder includes a (meth)acrylic acid ester monomer unit, a (meth)acrylonitrile monomer unit, an acid group-containing monomer unit, a (meth)acrylamide monomer unit and a crosslinkable monomer.
- the (meth)acrylic acid ester monomer that can be used for preparing the polymer as the binder is preferably a fluorine-free (meth)acrylic acid ester monomer. That is, the (meth)acrylic acid ester monomer units that can be contained in the polymer as the binder are preferably fluorine-free (meth)acrylic acid ester monomer units.
- the ratio of (meth)acrylic acid ester monomer units in the polymer as a binder is not particularly limited, but the total repeating units (total monomer units) contained in the polymer is 100% by mass, for example 40 mass % or more, may be 50 mass % or more, may be 60 mass % or more, and may be, for example, 90 mass % or less, and may be 85 mass % or less.
- the ratio of (meth)acrylonitrile monomer units in the polymer as a binder is not particularly limited, but is, for example, 1% by mass or more when the total repeating units (total monomer units) contained in the polymer is 100% by mass. and may be 5% by mass or more, or 10% by mass or more, for example, 20% by mass or less, and may be 15% by mass or less.
- the ratio of the acid group-containing monomer units in the polymer used as the binder is not particularly limited, but is, for example, 0.5% by mass based on 100% by mass of all repeating units (total monomer units) contained in the polymer. 1% by mass or more, 2% by mass or more, for example, 10% by mass or less, 7% by mass or less, or 5% by mass or less.
- the ratio of the (meth)acrylamide monomer unit in the polymer as the binder is not particularly limited, but is, for example, 0.1 mass when the total repeating units (total monomer units) contained in the polymer is 100% by mass. % or more, may be 0.5% by mass or more, may be 1% by mass or more, may be, for example, 5% by mass or less, may be 4% by mass or less, or may be 2% by mass or less.
- the ratio of the aromatic vinyl monomer units in the polymer as the binder is not particularly limited, but is, for example, 20% by mass or more, with the total repeating units (total monomer units) contained in the polymer being 100% by mass. It may be 40% by mass or more, or 55% by mass or more, for example, 80% by mass or less, 70% by mass or less, or 65% by mass or less.
- the (meth)acrylic acid ester monomer unit having a polar group in the polymer as the binder is not particularly limited. It is 0.1% by mass or more, and may be 0.5% by mass or more, for example, 3% by mass or less, and may be 1.5% by mass or less.
- the ratio of the crosslinkable monomer units in the polymer as the binder is not particularly limited, but is, for example, 1% by mass or more when the total repeating units (total monomer units) contained in the polymer is 100% by mass. , 2% by mass or more, or 3% by mass or more, for example, 50% by mass or less, 40% by mass or less, or 35% by mass or less.
- the ratio of the crosslinkable monomer unit in the polymer is not particularly limited, but the total amount contained in the polymer
- the repeating unit (total monomer unit) is 100% by mass, for example, 1% by mass or more, 2% by mass or more, or 3% by mass or more, for example, 6% by mass or less, or even 5% by mass or less. Well, it may be 4% by mass or less.
- the ratio of the crosslinkable monomer unit in the polymer is not particularly limited, but is included in the polymer
- the total repeating unit (total monomer unit) is 100% by mass, for example, it is 10% by mass or more, may be 20% by mass or more, or may be 30% by mass or more, for example, 50% by mass or less, and 40% by mass or less. or 35% by mass or less.
- the volume average particle diameter of the particulate binder is preferably 50 nm or more, more preferably 100 nm or more, further preferably 200 nm or more, and 600 nm or less. , more preferably 500 nm or less, and even more preferably 400 nm or less. If the volume-average particle size of the particulate binder is within the above range, the battery members can be more strongly adhered to each other via the adhesive material.
- the amount of the binder is not particularly limited, but is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and 20 parts by mass or less per 100 parts by mass of the particulate polymer. is preferred, and 15 parts by mass or less is more preferred. If the blending amount of the binder is within the above range, the cycle characteristics of the secondary battery can be improved while sufficiently preventing the components contained in the adhesive layer from coming off.
- the adhesive layer composition may not contain a binder. If it does not contain a binder, the increase in internal resistance can be suppressed and the cycle characteristics can be further improved.
- the polymer as the binder preferably has a water contact angle of 10° or more, more preferably 15° or more, preferably 90° or less, and more preferably 80° or less. . If the water contact angle is within the above range, the particulate binder can have good hydrophobicity, and as a result, the dispersibility of the particulate binder in the adhesive layer composition can be improved. Also, the particulate binder can interact well with polyalkylene glycol.
- the "water contact angle" is obtained by coating an aqueous dispersion or aqueous solution of a binder on a separator substrate, and 2 microliters of ion-exchanged water is dropped on the surface of a layer composed of a polymer as a binder.
- the contact angle meter manufactured by Kyowa Interface Science Co., Ltd., "PCA-1" can be used to measure the droplet after 1 second.
- the polymer as the binder is not particularly limited, and can be prepared, for example, by polymerizing a monomer composition containing the monomers described above in an aqueous solvent such as water.
- the proportion of each monomer in the monomer composition is usually the same as the proportion of each monomer unit in the polymer.
- the polymerization method and polymerization reaction are not particularly limited, and known polymerization methods and polymerization reactions can be used.
- a low-molecular-weight polyhydric alcohol compound is a compound having a molecular weight of less than 150 and two or more hydroxyl groups (—OH) in one molecule.
- the low-molecular-weight polyhydric alcohol compound having multiple hydroxyl groups in one molecule functions as a wetting agent, and the water in the adhesive layer composition evaporates in the nozzle (particularly, the supply It is thought that this is because it is possible to suppress the vaporization of water in the nozzle during the standing time when the is temporarily interrupted, and as a result, it is possible to suppress the deposition of the adhesive material such as the particulate polymer.
- examples of low-molecular-weight polyhydric alcohol compounds include propylene glycol, ethylene glycol, glycerin, 1,3-propanediol, and 1,4-butanediol.
- glycerin is preferred.
- One of these may be used alone, or two or more of them may be used in combination at any ratio.
- the content of the low molecular weight polyhydric alcohol compound per 100 parts by mass of the particulate polymer is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 50 parts by mass or more. Preferably, it is 55 parts by mass or more, preferably 400 parts by mass or less, more preferably 300 parts by mass or less, even more preferably 250 parts by mass or less, and 200 parts by mass or less. is even more preferred.
- the content of the low-molecular-weight polyhydric alcohol compound is at least the above lower limit, the inkjet ejection characteristics can be further improved.
- the content of the low-molecular-weight polyhydric alcohol compound is equal to or less than the upper limit, excessive increase in viscosity of the adhesive layer composition can be suppressed, and as a result, the inkjet ejection characteristics can be further improved.
- the content of the low-molecular-weight polyhydric alcohol compound per 100 parts by mass of water is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. It is preferably no more than 50 parts by mass, more preferably no more than 29 parts by mass.
- the content of the low-molecular-weight polyhydric alcohol compound is at least the above lower limit, the inkjet ejection characteristics can be further improved.
- the content of the low-molecular-weight polyhydric alcohol compound is equal to or less than the upper limit, excessive increase in viscosity of the adhesive layer composition can be suppressed, and as a result, the inkjet ejection characteristics can be further improved.
- the adhesive layer composition of the present invention preferably further contains a water-soluble polymer as a dispersant. If the composition for the adhesive layer contains a water-soluble polymer as a dispersant, the inkjet discharge characteristics, the adhesion between the electrode members of the secondary battery, the electrolyte pourability of the secondary battery, and the cycle characteristics of the secondary battery can be improved. can improve.
- the adhesive layer composition of the present invention may contain a dispersant other than the water-soluble polymer.
- the polymer being "water-soluble” means that the insoluble matter is less than 1.0% by mass when 0.5 g of the polymer is dissolved in 100 g of water at 25°C. .
- a substance whose solubility changes depending on the pH of water is considered to be "water-soluble” if it corresponds to the above-mentioned "water-soluble” at least at any pH.
- water-soluble polymers include, but are not limited to, ammonium acrylate polymers, polyacrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; copolymers of acrylic acid or acrylate and vinyl alcohol. fully or partially saponified maleic anhydride or copolymer of maleic acid or fumaric acid and vinyl acetate; modified polyvinyl alcohol; modified polyacrylic acid; polycarboxylic acid; ethylene-vinyl alcohol copolymer; ; an acrylamide polymer into which a carboxylic acid group and/or a cyano group has been introduced; Among these, ammonium acrylate-based polymers and polyacrylates such as sodium polyacrylate are preferred.
- ammonium acrylate-based polymers and polyacrylates such as sodium polyacrylate are preferred.
- the content of the dispersant per 100 parts by mass of the particulate polymer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and preferably 5 parts by mass or less. It is more preferably 2 parts by mass or less.
- the content of the dispersant is at least the lower limit, the dispersibility of the particulate polymer in the adhesive layer composition can be improved.
- the content of the dispersant is equal to or less than the upper limit, the inkjet ejection characteristics can be improved.
- the thixotropic agent is a component that imparts viscosity to the adhesive layer composition. Further, since the thixotropic agent has adhesiveness and electrolyte resistance, it can play a role of assisting adhesion between components in the adhesive layer composition and between battery members in the secondary battery.
- a thixotropic agent is generally a polymer having a number average molecular weight of 10,000 or more.
- the thixotropic agent is not particularly limited, but known substances such as natural polymers, semi-synthetic polymers and synthetic polymers can be used. Among these, the thixotropic agent is preferably carboxymethyl cellulose (CMC) and salts thereof, and cellulose nanofiber (CNF).
- CMC carboxymethyl cellulose
- CNF cellulose nanofiber
- the content of the thixotropic agent per 100 parts by mass of the particulate polymer is preferably 0.05 parts by mass or more, preferably 5 parts by mass or less, and more preferably, from the viewpoint of ensuring good battery characteristics of the secondary battery. is 1 part by mass or less, more preferably 0.4 parts by mass or less.
- the method for preparing the non-aqueous secondary battery adhesive layer composition of the present invention is not particularly limited.
- the stirring and mixing method is not particularly limited, and can be carried out by a known method. Specifically, general stirring vessels, ball mills, sand mills, bead mills, pigment dispersers, ultrasonic dispersers, crushing machines, homogenizers, planetary mixers, Filmix, and the like can be used.
- the mixing conditions are not particularly limited, the mixing can usually be carried out at room temperature or higher and 80° C. or lower for 10 minutes or longer and several hours or shorter.
- the adhesive layer for non-aqueous secondary batteries of the present invention is obtained using the composition for non-aqueous secondary battery adhesive layers of the present invention. Moreover, the adhesive layer for non-aqueous secondary batteries of the present invention functions as an adhesive material for bonding battery members used in non-aqueous secondary batteries.
- the adhesive layer for non-aqueous secondary batteries of the present invention can be obtained, for example, by the method for producing an adhesive layer for non-aqueous secondary batteries of the present invention, which will be described later.
- the adhesive layer for non-aqueous secondary batteries of the present invention is a dried product obtained by drying the composition for non-aqueous secondary battery adhesive layers of the present invention.
- the adhesive layer for a non-aqueous secondary battery of the present invention contains at least the particulate polymer and polyalkylene glycol described above, and optionally contains the other components described above. Since the adhesive layer for a non-aqueous secondary battery of the present invention uses the composition for a non-aqueous secondary battery adhesive layer of the present invention, it imparts excellent electrolyte pourability to the non-aqueous secondary battery, and is non-aqueous. It is possible to provide an aqueous secondary battery with excellent adhesion between battery members, and to exhibit excellent cycle characteristics in a non-aqueous secondary battery.
- the particulate polymer exists in the form of particles in the adhesive layer composition, but may be in the form of particles in the adhesive layer, or may be in any other shape.
- the shape of the adhesive layer is not particularly limited, and can be formed to have any planar shape such as stripes, dots, lattices, and the like. Above all, from the viewpoint of reducing the resistance of the secondary battery, it is preferable to form the adhesive layer in a dot shape.
- the dot-shaped adhesive layer can be obtained, for example, by an inkjet method using a coating machine (51 to 54 in FIG. 2) described later.
- the diameter of the dots of the adhesive layer arranged in a dot pattern is preferably 10 ⁇ m or more, more preferably 20 ⁇ m or more, preferably 300 ⁇ m or less, and more preferably 200 ⁇ m or less. If the dot diameter of the adhesive layer is equal to or greater than the above lower limit, the adhesive strength between the battery members can be enhanced. On the other hand, when the dot diameter of the adhesive layer is equal to or less than the above upper limit, it is possible to suppress deterioration of the output characteristics of the secondary battery.
- the thickness of the dots of the adhesive layer arranged in a dot pattern is preferably 5 ⁇ m or more.
- the dot thickness of the adhesive layer is equal to or greater than the above lower limit, the adhesive strength between the battery members can be enhanced.
- the basis weight of the adhesive layer is preferably 0.02 g/m 2 or more, preferably 1.0 g/m 2 or less, and more preferably 0.35 g/m 2 or less.
- the basis weight of the adhesive layer is at least the above lower limit, it is possible to ensure sufficient adhesive strength between the battery members.
- the basis weight of the adhesive layer is equal to or less than the above upper limit, sufficiently high output characteristics of the secondary battery can be ensured.
- the coverage of the adhesive layer is preferably 1% or more, more preferably 5% or more, preferably 50% or less, and more preferably 30% or less.
- the coverage of the adhesive layer is equal to or higher than the above lower limit, it is possible to ensure the adhesive strength between the battery members.
- the coverage of the adhesive layer is equal to or less than the above upper limit, sufficiently high output characteristics of the secondary battery can be ensured.
- the "adhesive layer coverage" in a certain surface or region means the ratio of the area of the portion covered with the adhesive layer to the total area of the surface or region [(area of the part covered with the adhesive layer / area of the entire surface or region) ⁇ 100 (%)].
- the "adhesive layer” in the “adhesive layer coverage” refers to the dried product of the adhesive layer composition. Point.
- the battery member for a non-aqueous secondary battery of the present invention comprises a substrate and the adhesive layer for a non-aqueous secondary battery of the present invention provided on the substrate, and the substrate is an electrode substrate or a separator It is the base material.
- the battery member for non-aqueous secondary batteries of the present invention can be obtained, for example, by the method for producing the battery member for non-aqueous secondary batteries of the present invention, which will be described later.
- the battery member for a non-aqueous secondary battery of the present invention includes the adhesive layer for a non-aqueous secondary battery of the present invention, it imparts excellent electrolyte pourability to the non-aqueous secondary battery, It can impart excellent adhesion between battery members to each other and allow the non-aqueous secondary battery to exhibit excellent cycle characteristics.
- the electrode base material includes a current collector and an electrode mixture layer provided on the current collector.
- an electrode made of an electrode base material in which an electrode mixture layer is formed on one or both sides of a current collector, or a porous membrane layer is further formed on the electrode mixture layer of the electrode base material. can be used.
- the current collector, the electrode mixture layer and the porous film layer are not particularly limited, and any collector that can be used in the field of secondary batteries, such as those described in JP-A-2013-145763, can be used. Electrical bodies, electrode composite layers and porous membrane layers may be used.
- the separator substrate is not particularly limited, and known separators such as organic separator substrates can be used.
- the organic separator base material is a porous member made of an organic material.
- organic separator substrates include polyolefin resins such as polyethylene and polypropylene, microporous membranes and nonwoven fabrics containing aromatic polyamide resins, etc. Polyethylene microporous membranes and nonwoven fabrics are preferred because of their excellent strength.
- a heat-resistant separator obtained by coating a ceramic on the separator is preferable.
- the separator base material may have a porous membrane layer formed on one side or both sides thereof.
- the porous membrane layer refers to a layer containing non-conductive particles as described in JP-A-2013-145763, for example.
- the method for producing a battery member for a non-aqueous secondary battery of the present invention includes a step of applying the non-aqueous secondary battery adhesive layer composition of the present invention onto an electrode base material or a separator base material by an inkjet method (coating step) and a step (drying step) of drying the non-aqueous secondary battery adhesive layer composition applied on the electrode base material or the separator base material.
- the coating step droplets of the adhesive layer composition of the present invention are applied onto an electrode base material or a separator base material through a nozzle of an inkjet coating machine.
- a conventionally known inkjet type coating machine can be used, and for example, coating can be performed using a coating machine (51 to 54 in FIG. 2) described later.
- the adhesive layer composition is preferably applied onto the electrode base material or the separator base material. It is preferable to apply to Further, it is more preferable to apply the adhesive layer composition onto the electrode mixture layer of the electrode substrate.
- the adhesive layer composition of the present invention has improved thickening properties due to polyalkylene glycol, even if the adhesive layer composition is applied onto the electrode mixture layer of the electrode substrate, the electrode mixture layer This is because impregnation of the adhesive layer composition into the inside is suppressed.
- the coating conditions by the inkjet method are not particularly limited as long as the adhesive layer composition can be coated on the substrate, and the desired form of the resulting adhesive layer (plan view shape, dot diameter, dot thickness , dot pitch, coverage, basis weight, etc.).
- Electrode base material and separator base material are not particularly limited, and known electrode base materials and separator base materials can be used.
- the electrode base material and the separator base material described above in the section "Battery member for non-aqueous secondary battery” can be used.
- the adhesive layer composition coated on the substrate is dried to form an adhesive layer made of the dried adhesive layer composition on the substrate.
- the drying method is not particularly limited, and a known method can be used. Examples of the drying method include a drying method using a heating device such as a heater, a dryer, and a heat roller.
- the drying conditions are not particularly limited, the drying temperature is preferably 50° C. or higher and 90° C. or lower, and the drying time is preferably 1 second or longer and 120 seconds or shorter.
- the laminate for a non-aqueous secondary battery of the present invention comprises an electrode and a separator, and the electrode and the separator are adhered via the adhesive layer for a non-aqueous secondary battery of the present invention.
- the electrode and the separator are bonded via the adhesive layer for non-aqueous secondary batteries of the present invention. It can provide the non-aqueous secondary battery with excellent adhesiveness between battery members, and can exhibit excellent cycle characteristics in the non-aqueous secondary battery.
- the electrode that is bonded to the separator to form the laminate may be only the positive electrode, only the negative electrode, or both the positive electrode and the negative electrode.
- the number of the positive electrode, the negative electrode, and the separator included in the laminate may be one, or two or more. good. That is, the structure of the laminate of the present invention may be any of the following (1) to (6).
- a plurality of positive electrodes and negative electrodes are separators Structure alternately laminated via (for example, "separator / negative electrode / separator / positive electrode / separator / negative electrode / separator / positive electrode” etc.)
- the electrode is not particularly limited, and known electrodes can be used. For example, those described in the section "Battery member for non-aqueous secondary battery” can be used.
- the separator is not particularly limited, and known separators can be used. For example, those described in the section "Battery member for non-aqueous secondary battery” can be used.
- the adhesive layer that bonds the electrode and the separator is a dried product of the adhesive layer composition for a non-aqueous secondary battery of the present invention. That is, the dried product contains at least the polymer derived from the particulate polymer and the polymer derived from the polyalkylene glycol, and optionally the other components described above.
- the preferred form of the adhesive layer (dot diameter, dot thickness, dot pitch, coverage, basis weight, etc.) is the same as described in the section "Adhesive layer for non-aqueous secondary battery".
- the particulate polymer exists in the form of particles in the adhesive layer composition, it may be in the form of particles or in any other shape in the adhesive layer of the laminate. .
- the method for producing a laminate for a non-aqueous secondary battery of the present invention includes a step of supplying an adhesive material to at least one bonding surface of an electrode and a separator (that is, a surface for forming an adhesive material (adhesive layer)) (supplying step), and a step of pressurizing and bonding the electrode and the separator via the bonding surface to which the adhesive material is supplied (bonding step).
- the manufacturing method of the laminate for a non-aqueous secondary battery of the present invention may include a step of cutting the obtained laminated body (cutting step) after the bonding step.
- the adhesive material is supplied to the bonding surface of at least one of the electrodes (positive electrode, negative electrode) and the separator.
- Supply of the adhesive material is not particularly limited.
- the adhesive layer composition of the present invention can be applied by an inkjet method and dried.
- the adhesive material may be supplied by transferring (laminating) an adhesive layer obtained by peeling from the release substrate onto the bonding surface.
- the release base material is not particularly limited, and known ones can be used.
- the conditions of the inkjet method are not particularly limited as long as the adhesive layer composition can be applied, and the desired form of the obtained adhesive material (plan view shape, dot diameter, dot thickness, dot pitch, coating ratio, basis weight, etc.).
- the electrode and the separator are transported to the bonding start position without contacting other members to the bonding surface to which the adhesive layer composition is supplied.
- the adhesive layer composition may be dried therein. Problems such as blocking do not occur unless another member is brought into contact with the bonding surface to which the adhesive layer composition has been supplied, so that the laminate can be produced efficiently.
- drying does not have to be performed.
- the "bonding start position" refers to a position at which the bonding surface of the electrode and the bonding surface of the separator are brought into contact when bonding the electrode and the separator.
- the transport of the electrodes and separators is not particularly limited, and can be performed using any transport mechanism such as rollers, belt conveyors, manipulators, and suction bands. Above all, from the viewpoint of further increasing the production efficiency of the laminate, it is preferable to convey at least one of the electrodes and the separator using rollers.
- drying of the adhesive layer composition is not particularly limited, and can be performed using a heating device such as a heater, a dryer, or a heat roller.
- the temperature at which the electrode and/or the separator supplied with the adhesive layer composition is dried is not particularly limited, but is preferably 50° C. or higher and 90° C. or lower.
- the drying time is not particularly limited, it is preferably 1 second or more and 120 seconds or less.
- the electrode and the separator are bonded together via the bonding surface.
- the lamination is performed by applying pressure to the laminated body of the electrode and the separator which are superimposed via the lamination surface.
- the pressing temperature of the laminate is not particularly limited as long as it is a temperature at which the electrode and the separator can be bonded together. , preferably 35° C. or lower, more preferably 30° C. or lower, and still more preferably 25° C. or lower.
- the pressure temperature of the laminate is equal to or higher than the above lower limit, the adhesiveness between the battery members can be improved.
- the pressing temperature of the laminate is equal to or lower than the above upper limit, the production efficiency of the laminate can be enhanced.
- the laminate is pressurized at a pressure of preferably 0.1 MPa or higher, more preferably 0.5 MPa or higher, and preferably 5 MPa or lower. If the laminate is pressed at a pressure equal to or higher than the above lower limit, the adhesiveness between the battery members can be improved. On the other hand, if the laminate is pressurized at a pressure equal to or lower than the upper limit, deformation of the laminate (such as crushing of the electrode mixture layer and the separator) can be effectively suppressed.
- the pressurization time of the laminate is preferably 20 seconds or less, more preferably 15 seconds or less. If the pressurization time of the laminate is equal to or less than the above upper limit, the production efficiency of the laminate can be enhanced.
- the cutting step is a step of cutting the bonded body obtained in the bonding step into desired dimensions.
- any cutting machine that can be used in the field of manufacturing secondary batteries such as a cutting machine that cuts the bonded body by sandwiching the bonded body with cutting blades from both sides in the thickness direction, can be used.
- Electrode and separators are not particularly limited, and known electrodes and separators can be used.
- the electrodes and separators described above in the section "Method for producing adhesive layer for non-aqueous secondary battery” can be used.
- the adhesive material for bonding the electrode and the separator is a dried product of the adhesive layer composition for non-aqueous secondary batteries of the present invention. That is, the dried product contains at least the polymer derived from the particulate polymer and the polymer derived from the polyalkylene glycol, and optionally the other components described above.
- the preferred form of the adhesive material (dot diameter, dot thickness, dot pitch, coverage, basis weight, etc.) is the same as described in the section "Adhesive layer for non-aqueous secondary battery".
- the particulate polymer is present in the form of particles in the non-aqueous secondary battery adhesive layer composition, but may be in the form of particles in the adhesive material (adhesion layer) in the laminate after pressurization. but may be of any other shape.
- a long first separator material roll 10A unwound from the first separator material roll is applied to one surface of the negative electrode material consisting of the long negative electrode material roll 20A unwound from the negative electrode material roll. are pasted together via an adhesive material supplied from the coating machine 51 .
- the long second separator raw roll 30A fed out from the second separator raw roll is applied via the adhesive material supplied from the coating machine 52. to paste together.
- bonding can be performed using pressure rollers 61 and 62, for example.
- the positive electrode 40 is attached to the surface of the first separator material 10A on the side opposite to the negative electrode material 20A side via the adhesive material supplied from the coating machine 53 at a predetermined arrangement pitch, and the positive electrode is attached. get a combination.
- the adhesive material is supplied from the coating machine 54 to the surface of the second separator material 30A opposite to the negative electrode material 20A side, and the bonded body is cut between the positive electrodes 40 adjacent in the longitudinal direction.
- a cutting machine 70 is used to cut the laminated body to obtain a laminate.
- the non-aqueous secondary battery of the present invention includes the non-aqueous secondary battery laminate of the present invention.
- the nonaqueous secondary battery of the present invention includes, for example, electrodes (a positive electrode and a negative electrode), an electrolytic solution, and a separator. Then, at least one of the positive electrode and the negative electrode and the separator are laminated via the adhesive layer for non-aqueous secondary batteries of the present invention to form the laminate for non-aqueous secondary batteries of the present invention. Since the non-aqueous secondary battery of the present invention includes the laminate for a non-aqueous secondary battery of the present invention, it is excellent in electrolyte pourability, adhesiveness between battery members, and cycle characteristics.
- the electrode used in the secondary battery of the present invention is not particularly limited, and known electrodes can be used, for example, those described in the section "Battery member for non-aqueous secondary battery” can be used.
- the separator used in the secondary battery of the present invention is not particularly limited, and known separators can be used, for example, those described in the section "Battery member for non-aqueous secondary battery” can be used.
- an organic electrolytic solution in which a supporting electrolyte is dissolved in an organic solvent is usually used.
- a lithium salt is used as the supporting electrolyte.
- lithium salts include LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , CF 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi. , (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 ) NLi and the like.
- LiPF 6 , LiClO 4 and CF 3 SO 3 Li are preferable, and LiPF 6 is particularly preferable, because they are easily dissolved in a solvent and exhibit a high degree of dissociation.
- one electrolyte may be used alone, or two or more electrolytes may be used in combination at an arbitrary ratio.
- Lithium ion conductivity usually tends to increase as a supporting electrolyte with a higher degree of dissociation is used, so lithium ion conductivity can be adjusted by the type of supporting electrolyte.
- the organic solvent used in the electrolytic solution is not particularly limited as long as it can dissolve the supporting electrolyte.
- Examples include dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC ), butylene carbonate (BC), ethyl methyl carbonate (EMC); esters such as ⁇ -butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur compounds; and the like are preferably used.
- DMC dimethyl carbonate
- EC ethylene carbonate
- DEC diethyl carbonate
- PC propylene carbonate
- BC butylene carbonate
- EMC ethyl methyl carbonate
- esters such as ⁇ -butyrolactone and methyl formate
- ethers such as 1,2-dimethoxyethane and tetrahydrofuran
- sulfur compounds and the like
- carbonates are preferably used because they have a high dielectric constant and a wide stable potential range, and a mixture of ethylene carbonate and ethyl methyl carbonate is more preferably used.
- known additives such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), ethyl methyl sulfone, and the like may be added to the electrolytic solution.
- a laminated body obtained by laminating a laminated body is rolled or folded according to the shape of the battery, and placed in a device container (battery container), It can be produced by injecting an electrolytic solution into a device container and sealing the container.
- the layered body the layered body itself may be used, or a plurality of layered bodies may be layered to be manufactured.
- the laminated body may be produced by laminating a laminated body and additional battery members (electrodes and/or separators, etc.).
- the secondary battery of the present invention may optionally contain a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, or the like. may be provided.
- the shape of the secondary battery may be, for example, coin-shaped, button-shaped, sheet-shaped, cylindrical, rectangular, or flat.
- ⁇ Glass transition temperature> The aqueous dispersions of the particulate polymers or particulate binders prepared in Examples and Comparative Examples were each dried at 130° C. for 1 hour to prepare measurement samples. Weigh 10 mg of the measurement sample in an aluminum pan, and use a differential thermal analysis measuring device ("EXSTAR DSC6220" manufactured by SII Nanotechnology Co., Ltd.) to measure the temperature range from -100 ° C. to 200 ° C., at a heating rate of 10 ° C./ Minutes, the measurement was performed under the conditions specified in JIS Z8703 to obtain a differential scanning calorimetry (DSC) curve. An empty aluminum pan was used as a reference.
- EXSTAR DSC6220 manufactured by SII Nanotechnology Co., Ltd.
- volume average particle size The volume average particle diameters of the particulate polymers and particulate binders prepared in Examples and Comparative Examples were measured by a laser diffraction method. Specifically, an aqueous dispersion solution (solid content concentration 0.1% by mass) containing the prepared particulate polymer or particulate binder was used as a sample, and a laser diffraction particle size distribution measuring device (manufactured by Beckman Coulter, product In the particle size distribution (volume basis) obtained by the name “LS-13 320”), the particle size at which the cumulative volume calculated from the small size side becomes 50% was obtained, and the volume average particle size D50 (nm) was obtained.
- a laser diffraction particle size distribution measuring device manufactured by Beckman Coulter, product In the particle size distribution (volume basis) obtained by the name “LS-13 320”
- ⁇ Number average molecular weight> The polyalkylene glycol used in Examples and Comparative Examples was diluted with water to adjust the concentration to 0.05%. Then, it was filtered through a 0.45 ⁇ m membrane filter made of PTFE to obtain a sample. This sample was analyzed by gel permeation chromatography under the following conditions to determine the number average molecular weight of polyalkylene glycol.
- Apparatus Gel permeation chromatograph GPC (manufactured by Agilent, product name "1260 In infinity II HPLC") Detector: Differential refractive index detector RI (manufactured by Agilent, product name "1260 Infin ity II RI detector”) Column: 2 TSKgel GMPWXL ( ⁇ 7.8 mm ⁇ 30 cm, manufactured by Tosoh) Solvent: 0.1 M Tris buffer (pH 9, 0.1 M potassium chloride added) Flow rate: 0.7 mL/min Column temperature: 40°C Injection volume: 0.2 mL Standard sample: Tosoh and Sigma-Aldrich, monodisperse polyethylene oxide
- ⁇ Inkjet ejection characteristics> For the non-aqueous secondary battery adhesive layer composition produced in each example and comparative example, a discharge experiment kit (IJK-200S, Microjet) equipped with a high-performance glass nozzle head (IJHD-100, manufactured by Microjet) (manufactured) was used to conduct a discharge test. Then, the ejection characteristics were evaluated according to the following criteria.
- peel strength is 5.0 N / m or more
- B Peel strength is 3.0 N / m or more and less than 5.0 N / m
- C Peel strength is 1.0 N / m or more and less than 3.0 N / m
- D Peel strength is Less than 1.0N/m
- the lithium ion secondary batteries produced in each example and comparative example were charged to 4.3 V by constant current and constant voltage (CC CV) in an atmosphere at a temperature of 25° C. to prepare cells.
- the prepared cell was discharged to 3.0 V by a constant current method of 0.2 C and 1 C in an atmosphere of -10° C. to determine the electric capacity.
- the lithium ion secondary battery was fastened with a pressurizing jig so as to have a surface pressure of 1 MPa, and then a cycle test was performed at 45°C.
- the cycle test conditions were 1C CC+CV charge (4.3V, 1/50C cut) and 1C CC discharge (3.0V cut), and the charge/discharge cycle was repeated 500 times.
- the temperature was lowered to 25° C. while the pressure jig was still fastened, and the output characteristics were measured in the same manner as described above.
- Example 1 Preparation of particulate polymer> 100 parts of ion-exchanged water and 0.1 part of ammonium persulfate were supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen gas, and the temperature was raised to 80°C.
- an aqueous dispersion containing the particulate polymer constituting the core portion was obtained.
- 60 parts of a shell-forming monomer composition containing 4.75 parts of styrene as an aromatic vinyl monomer and 0.25 parts of methacrylic acid as an acid group-containing monomer was added to this aqueous dispersion. It was continuously supplied over a period of minutes to continue the polymerization.
- the reaction was stopped by cooling to prepare an aqueous dispersion containing a particulate polymer.
- the volume average particle size and glass transition temperature of the obtained particulate polymer were measured. Table 1 shows the results. Further, by observing the cross-sectional structure of the particulate polymer using a transmission electron microscope (TEM), the particulate polymer has a core-shell structure in which the shell portion partially covers the outer surface of the core portion. It was confirmed.
- TEM transmission electron microscope
- ⁇ Preparation of non-aqueous secondary battery adhesive layer composition 100 parts of an aqueous dispersion of a particulate polymer equivalent to solid content, 60 parts of polyethylene glycol 600 (number average molecular weight: 600) as a polyalkylene glycol, 60 parts of glycerin as a low molecular weight polyhydric alcohol, Add 1 part of ammonium acrylate polymer (Toagosei Co., Ltd., Aron (registered trademark) A-6114) as a dispersant (water-soluble polymer) in terms of solid content, and add 1779 parts of ion-exchanged water.
- a composition for a non-aqueous secondary battery adhesive layer was obtained. Then, using the obtained composition for a non-aqueous secondary battery adhesive layer, the inkjet discharge characteristics and the dry adhesiveness were evaluated. Table 1 shows the results.
- ⁇ Preparation of negative electrode original fabric 33 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 63.5 parts of styrene, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and polymerization initiation are placed in a 5 MPa pressure vessel equipped with a stirrer. After 0.5 part of potassium persulfate was added as an agent and sufficiently stirred, the mixture was heated to 50° C. to initiate polymerization. When the polymerization conversion reached 96%, the mixture was cooled to stop the reaction, and a mixture containing the binder for the negative electrode mixture layer (SBR) was obtained.
- SBR negative electrode mixture layer
- a 5% aqueous sodium hydroxide solution was added to the mixture containing the binder for the negative electrode mixture layer to adjust the pH to 8, and unreacted monomers were removed by heating under reduced pressure distillation. Thereafter, the mixture was cooled to a temperature of 30° C. or lower to obtain an aqueous dispersion containing the desired binder for the negative electrode mixture layer.
- 100 parts of artificial graphite (volume average particle size: 15.6 ⁇ m) as a negative electrode active material and a 2% aqueous solution of carboxymethyl cellulose sodium salt (manufactured by Nippon Paper Industries, product name “MAC350HC”) as a viscosity modifier are solidified.
- the mixture was further mixed at a temperature of 25° C. for 60 minutes. Furthermore, after adjusting the solid content concentration to 62% with ion-exchanged water, the mixture was further mixed at a temperature of 25° C. for 15 minutes. 1.5 parts of the aqueous dispersion containing the binder for the negative electrode mixture layer and ion-exchanged water were added to the resulting mixture so that the final solid concentration was 52%. Adjusted and mixed for an additional 10 minutes. This was defoamed under reduced pressure to obtain a highly fluid slurry composition for a non-aqueous secondary battery negative electrode.
- the obtained slurry composition for a non-aqueous secondary battery negative electrode is coated with a comma coater on both sides of a copper foil having a thickness of 20 ⁇ m as a current collector so that the film thickness after drying is about 150 ⁇ m, dried.
- This drying was carried out by conveying the copper foil at a speed of 0.5 m/min in an oven at a temperature of 60° C. for 2 minutes. After that, heat treatment was performed at a temperature of 120° C. for 2 minutes to obtain a negative electrode raw sheet before pressing.
- the negative electrode raw material before pressing was rolled by a roll press to obtain a negative electrode raw material after pressing in which the thickness of the negative electrode mixture layer was 80 ⁇ m.
- ⁇ Preparation of positive electrode original sheet 100 parts of LiCoO 2 having a volume average particle diameter of 12 ⁇ m as a positive electrode active material, 2 parts of acetylene black (manufactured by Denka Co., Ltd., product name “HS-100”) as a conductive material, and polyfluoride as a binder. 2 parts of vinylidene (manufactured by Kureha Co., Ltd., product name "#7208”) was mixed with N-methylpyrrolidone as a solvent to adjust the total solid concentration to 70%. These were mixed by a planetary mixer to obtain a slurry composition for non-aqueous secondary battery positive electrode.
- the obtained slurry composition for a non-aqueous secondary battery positive electrode is coated on both sides of a 20 ⁇ m thick aluminum foil as a current collector with a comma coater so that the film thickness after drying is about 150 ⁇ m, dried.
- This drying was carried out by conveying the aluminum foil at a speed of 0.5 m/min through an oven at a temperature of 60° C. for 2 minutes. After that, heat treatment was performed at a temperature of 120° C. for 2 minutes to obtain a positive electrode original fabric. Then, the obtained positive electrode raw sheet was rolled using a roll press to obtain a positive electrode raw sheet after pressing including the positive electrode mixture layer.
- a raw separator sheet made of polyethylene (PE) (product name: “ND412” manufactured by Asahi Kasei Corporation) was prepared.
- a laminated body was produced as shown in FIG. 3 using the produced non-aqueous secondary battery adhesive layer composition, negative electrode original sheet, positive electrode original sheet and separator original sheet.
- reference numeral 91 denotes a conveying roller
- reference numeral 92 denotes a heat roller.
- an inkjet coating machine 52 Konica, KM1024 was applied onto one surface of the negative electrode raw roll 20A.
- the non-aqueous secondary battery adhesive layer composition is supplied from the inkjet head, and the second separator raw roll 30A and the negative electrode raw roll 20A fed out from the separator raw roll are pressed by pressure rollers 61 and 62. pasted together with
- a non-aqueous secondary battery adhesive layer composition is supplied from an inkjet head of an inkjet coating machine 51 (manufactured by Konica, KM1024 (sheer mode type)) onto the other surface of the negative electrode raw material 20A, and the separator The first separator material roll 10A fed out from the material roll and the laminate of the negative electrode material material 20A and the second separator material material 30A were bonded together by pressing rollers 61 and 62 .
- an adhesive layer composition is applied from an inkjet head of an inkjet coating machine 53 (manufactured by Konica, KM1024 (sheer mode type)).
- an inkjet coating machine 53 manufactured by Konica, KM1024 (sheer mode type)
- the laminate of the first separator material 10A, the negative electrode material 20A, and the second separator material 30A, and the positive electrode 40 are pressed with pressure rollers 61 and 62. pasted together.
- the adhesive layer composition onto the positive electrode 40 from the inkjet head of the inkjet coating machine 54 (manufactured by Konica, KM1024 (sheer mode type)), it is cut by the cutting machine 70 to form a second separator. , the negative electrode, the first separator, and the positive electrode were laminated in this order to obtain a laminate.
- portions where the electrode mixture layer (the positive electrode mixture layer or the negative electrode mixture layer) is not formed are provided at the end portions of the respective current collectors of the positive electrode 40 and the negative electrode raw sheet 20A.
- the tabs were punched out to form tabs of the same size, and lamination was performed so that the positive electrode tab and the negative electrode tab were arranged on the same edge side of the bonding surfaces X and Y between the electrode and the separator. Electrolyte pourability was evaluated using the obtained laminate. Table 1 shows the results.
- the bonding using the pressing rollers 61 and 62 was performed at a temperature of 25° C. and a pressure of 2 MPa. Further, the supplied adhesive layer composition was dried by using a heat roller 92 as part of the conveying roller 91 (drying temperature: 70° C., drying time: 1 second).
- the adhesive layer composition was supplied from the coating machines 51 to 54 so that the adhesive layer composition formed a uniform dot-like pattern.
- the dot size was 100 ⁇ m in diameter and the interval was 400 ⁇ m pitch.
- the basis weight of the adhesive material was 0.2 g/m 2 . Moreover, when the coverage was measured, it was 6.5%.
- Example 2 Various operations, measurements and evaluations were performed in the same manner as in Example 1, except that the aqueous dispersion containing the particulate polymer was obtained by the following preparation method. Table 1 shows the results.
- an aqueous dispersion containing the particulate polymer constituting the core portion was obtained.
- 60 parts of a shell-forming monomer composition containing 4.75 parts of styrene as an aromatic vinyl monomer and 0.25 parts of methacrylic acid as an acid group-containing monomer was added to this aqueous dispersion. It was continuously supplied over a period of minutes to continue the polymerization.
- the reaction was stopped by cooling to prepare an aqueous dispersion containing a particulate polymer having a core-shell structure.
- Example 3 Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the composition obtained by the following preparation method was used as the non-aqueous secondary battery adhesive layer composition. Table 1 shows the results.
- an aqueous dispersion containing the particulate polymer constituting the core portion was obtained.
- an aqueous dispersion containing the particulate polymer constituting the core portion was obtained.
- aqueous dispersion were added 4.7 parts of styrene as an aromatic vinyl monomer, 0.05 parts of methacrylic acid as an acid group-containing monomer, and 0.0 part of acrylonitrile as a (meth)acrylonitrile monomer. 25 parts of the shell-forming monomer composition was continuously supplied over 60 minutes to continue the polymerization.
- the reaction was stopped by cooling to prepare an aqueous dispersion containing a particulate polymer having a core-shell structure.
- ⁇ Preparation of particulate binder> A reactor equipped with a stirrer was charged with 90 parts of ion-exchanged water, 0.05 parts of sodium dodecylbenzenesulfonate (manufactured by Kao Chemical Co., Ltd., "Neopelex G-15") as an emulsifier, and 0.23 of ammonium persulfate. , respectively, the gas phase was replaced with nitrogen gas, and the temperature was raised to 70°C.
- This monomer composition was continuously added to the reactor over 4 hours to carry out polymerization.
- the reaction was carried out at 80° C. during the addition.
- the mixture was further stirred at 80° C. for 3 hours to complete the reaction, and an aqueous dispersion containing a particulate binder having no core-shell structure was prepared.
- ⁇ Preparation of non-aqueous secondary battery adhesive layer composition 100 parts of aqueous dispersion of particulate polymer, 10 parts of aqueous dispersion of particulate binder, 60 parts of polyethylene glycol 600 as polyalkylene glycol, 60 parts of glycerin as a functional alcohol and 1 part of solid content equivalent to an ammonium acrylate polymer (manufactured by Toagosei Co., Ltd., Aron (registered trademark) A-6114) as a dispersant (water-soluble polymer) are added. Then, 1769 parts of ion-exchanged water was added to obtain a non-aqueous secondary battery adhesive layer composition.
- Example 4 Various operations, measurements, and evaluations were performed in the same manner as in Example 3, except that the aqueous dispersion containing the particulate binder was prepared by the following preparation method. Table 1 shows the results.
- the monomer composition as a whole comprises 62.2 parts of styrene as the aromatic vinyl monomer, 33 parts of 1,3-butadiene as the crosslinkable monomer, and itaconic acid as the acid group-containing monomer. 3.8 parts and 1 part of 2-hydroxyethyl acrylate as a (meth)acrylic ester monomer having a polar group were used. After 5.5 hours from the initiation of the second-stage polymerization, the addition of the entire amount of the mixture containing these monomer compositions was completed, and then the mixture was further heated to 85° C. and reacted for 6 hours. When the polymerization conversion reached 97%, the reaction was terminated by cooling.
- a 5% sodium hydroxide aqueous solution was added to the mixture containing this polymer to adjust the pH to 8. Thereafter, unreacted monomers were removed by heating under reduced pressure distillation. After cooling, an aqueous dispersion containing a particulate binder having no core-shell structure was prepared.
- Example 5 Various operations, measurements and evaluations were performed in the same manner as in Example 1, except that polyethylene glycol 200 having a number average molecular weight of 200 was used in place of polyethylene glycol 600 in the preparation of the non-aqueous secondary battery adhesive layer composition. did Table 1 shows the results.
- Example 6 Various operations, measurements and evaluations were performed in the same manner as in Example 1, except that polypropylene glycol 400 having a number average molecular weight of 400 was used in place of polyethylene glycol 600 in the preparation of the non-aqueous secondary battery adhesive layer composition. did Table 1 shows the results.
- Example 7 Various operations, measurements and evaluations were performed in the same manner as in Example 1, except that polyethylene glycol 1000 having a number average molecular weight of 1000 was used in place of polyethylene glycol 600 in the preparation of the non-aqueous secondary battery adhesive layer composition. did Table 1 shows the results.
- non-aqueous secondary battery adhesive layer composition instead of polyethylene glycol 600, polyoxyethylene polyoxypropylene glycol having a number average molecular weight of 1102 (ADEKA Co., Ltd., ADEKA (registered trademark) Pluronic L-31) Various operations, measurements and evaluations were carried out in the same manner as in Example 1 except that the was used. Table 1 shows the results.
- polyethylene glycol 600 polyoxyethylene polyoxypropylene glycol having a number average molecular weight of 1102 (ADEKA Co., Ltd., ADEKA (registered trademark) Pluronic L-31)
- Example 9 Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that tetraethylene glycol monobutyl ether was used instead of polyethylene glycol 600 in the preparation of the non-aqueous secondary battery adhesive layer composition. Table 1 shows the results.
- Example 10 Except for changing the amount of polyethylene glycol 600 used to 20 parts, changing the amount of water used to 1817 parts, and using 2 parts of carboxymethyl cellulose as a thixotropic agent in the preparation of the non-aqueous secondary battery adhesive layer composition. performed various operations, measurements and evaluations in the same manner as in Example 1. Table 1 shows the results.
- Example 1 Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that diethylene glycol was used instead of polyethylene glycol 600 in the preparation of the non-aqueous secondary battery adhesive layer composition. Table 1 shows the results.
- BA indicates butyl acrylate
- MAA indicates methacrylic acid
- AN indicates acrylonitrile
- 2EHA denotes 2-ethylhexyl acrylate
- St indicates styrene
- EDMA indicates ethylene glycol dimethacrylate
- PEG indicates polyethylene glycicol
- PPG indicates polypropylene glycol
- EO-PO indicates polyoxyethylene polyoxypropylene glycol
- TGME indicates tetraethylene glycol monobutyl ether
- DEG indicates diethylene glycol
- CMC indicates carboxymethyl cellulose.
- the adhesive layer compositions of Examples 1 to 10 provided excellent electrolyte pourability to non-aqueous secondary batteries while ensuring inkjet ejection characteristics. It can be seen that excellent adhesion between battery members can be imparted to the secondary battery, and excellent cycle characteristics can be exhibited in the non-aqueous secondary battery.
- the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesiveness between battery members, and It is possible to provide a non-aqueous secondary battery adhesive layer composition capable of exhibiting excellent cycle characteristics in a non-aqueous secondary battery. Further, according to the present invention, the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesiveness between battery members, and the non-aqueous secondary battery It is possible to provide an adhesive layer for a non-aqueous secondary battery, a battery member for a non-aqueous secondary battery, and a laminate for a non-aqueous secondary battery that can exhibit excellent cycle characteristics.
- non-aqueous secondary battery that is excellent in electrolyte pourability, adhesion between battery members, and cycle characteristics. Further, according to the present invention, the non-aqueous secondary battery is provided with excellent electrolyte pourability, the non-aqueous secondary battery is provided with excellent adhesiveness between battery members, and the non-aqueous secondary battery It is possible to provide a method for manufacturing a battery member for a non-aqueous secondary battery and a method for manufacturing a laminate for a non-aqueous secondary battery, which can exhibit excellent cycle characteristics.
Landscapes
- Chemical & Material Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Electrochemistry (AREA)
- General Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Materials Engineering (AREA)
- Organic Chemistry (AREA)
- Secondary Cells (AREA)
- Battery Electrode And Active Subsutance (AREA)
Priority Applications (5)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202380015784.2A CN118476110A (zh) | 2022-02-28 | 2023-02-01 | 非水系二次电池黏合层用组合物、非水系二次电池用黏合层、非水系二次电池用电池构件及其制造方法、非水系二次电池用层叠体及其制造方法、以及非水系二次电池 |
| EP23759611.9A EP4489206A4 (en) | 2022-02-28 | 2023-02-01 | Composition of adhesive layer for non-aqueous secondary batteries, adhesive layer for non-aqueous secondary batteries, battery element for non-aqueous secondary batteries, process for producing the latter, laminate for non-aqueous secondary batteries, process for producing the latter, and non-aqueous secondary batteries |
| US18/835,350 US20250129274A1 (en) | 2022-02-28 | 2023-02-01 | Composition for non-aqueous secondary battery adhesive layer, adhesive layer for non-aqueous secondary battery, battery member for non-aqueous secondary battery and method of producing same, laminate for non-aqueous secondary battery and method of producing same, and non-aqueous secondary battery |
| JP2024502951A JPWO2023162605A1 (cg-RX-API-DMAC7.html) | 2022-02-28 | 2023-02-01 | |
| KR1020247027861A KR20240157660A (ko) | 2022-02-28 | 2023-02-01 | 비수계 이차 전지 접착층용 조성물, 비수계 이차 전지용 접착층, 비수계 이차 전지용 전지 부재 및 그 제조 방법, 비수계 이차 전지용 적층체 및 그 제조 방법, 그리고, 비수계 이차 전지 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022030463 | 2022-02-28 | ||
| JP2022-030463 | 2022-02-28 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023162605A1 true WO2023162605A1 (ja) | 2023-08-31 |
Family
ID=87765581
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/003271 Ceased WO2023162605A1 (ja) | 2022-02-28 | 2023-02-01 | 非水系二次電池接着層用組成物、非水系二次電池用接着層、非水系二次電池用電池部材及びその製造方法、非水系二次電池用積層体及びその製造方法、並びに、非水系二次電池 |
Country Status (6)
| Country | Link |
|---|---|
| US (1) | US20250129274A1 (cg-RX-API-DMAC7.html) |
| EP (1) | EP4489206A4 (cg-RX-API-DMAC7.html) |
| JP (1) | JPWO2023162605A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20240157660A (cg-RX-API-DMAC7.html) |
| CN (1) | CN118476110A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023162605A1 (cg-RX-API-DMAC7.html) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2026016535A1 (zh) * | 2024-07-15 | 2026-01-22 | 宁德时代新能源科技股份有限公司 | 金属电池和用电装置 |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2012060147A1 (ja) * | 2010-11-05 | 2012-05-10 | 東レ株式会社 | 複合多孔質膜及びその製造方法 |
| JP2013145763A (ja) | 2013-04-30 | 2013-07-25 | Nippon Zeon Co Ltd | 二次電池多孔膜用スラリー組成物、二次電池用電極、二次電池用セパレータおよび二次電池 |
| JP2016025093A (ja) * | 2014-07-23 | 2016-02-08 | ラッキー フィルム カンパニー・リミテッド | スラリー組成物およびそれを含んでなるリチウムイオン電池用セパレータ |
| WO2020246497A1 (ja) * | 2019-06-04 | 2020-12-10 | 帝人株式会社 | 非水系二次電池用セパレータ及び非水系二次電池 |
Family Cites Families (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN112088446B (zh) * | 2018-05-17 | 2023-06-20 | 日本瑞翁株式会社 | 非水系二次电池用浆料、非水系二次电池用间隔件、非水系二次电池用电极、非水系二次电池用层叠体以及非水系二次电池 |
-
2023
- 2023-02-01 US US18/835,350 patent/US20250129274A1/en active Pending
- 2023-02-01 EP EP23759611.9A patent/EP4489206A4/en active Pending
- 2023-02-01 JP JP2024502951A patent/JPWO2023162605A1/ja active Pending
- 2023-02-01 CN CN202380015784.2A patent/CN118476110A/zh active Pending
- 2023-02-01 KR KR1020247027861A patent/KR20240157660A/ko active Pending
- 2023-02-01 WO PCT/JP2023/003271 patent/WO2023162605A1/ja not_active Ceased
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2012060147A1 (ja) * | 2010-11-05 | 2012-05-10 | 東レ株式会社 | 複合多孔質膜及びその製造方法 |
| JP2013145763A (ja) | 2013-04-30 | 2013-07-25 | Nippon Zeon Co Ltd | 二次電池多孔膜用スラリー組成物、二次電池用電極、二次電池用セパレータおよび二次電池 |
| JP2016025093A (ja) * | 2014-07-23 | 2016-02-08 | ラッキー フィルム カンパニー・リミテッド | スラリー組成物およびそれを含んでなるリチウムイオン電池用セパレータ |
| WO2020246497A1 (ja) * | 2019-06-04 | 2020-12-10 | 帝人株式会社 | 非水系二次電池用セパレータ及び非水系二次電池 |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP4489206A4 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2026016535A1 (zh) * | 2024-07-15 | 2026-01-22 | 宁德时代新能源科技股份有限公司 | 金属电池和用电装置 |
Also Published As
| Publication number | Publication date |
|---|---|
| KR20240157660A (ko) | 2024-11-01 |
| US20250129274A1 (en) | 2025-04-24 |
| JPWO2023162605A1 (cg-RX-API-DMAC7.html) | 2023-08-31 |
| EP4489206A4 (en) | 2026-03-18 |
| CN118476110A (zh) | 2024-08-09 |
| EP4489206A1 (en) | 2025-01-08 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7306272B2 (ja) | 非水系二次電池機能層用組成物、非水系二次電池用電池部材、非水系二次電池用積層体の製造方法、および非水系二次電池 | |
| JP7363777B2 (ja) | 非水系二次電池用スラリー、非水系二次電池用セパレータ、非水系二次電池用電極、非水系二次電池用積層体および非水系二次電池 | |
| JP7823656B2 (ja) | 非水系二次電池接着層用組成物、非水系二次電池用接着層およびその製造方法、非水系二次電池用積層体およびその製造方法、ならびに、非水系二次電池 | |
| JP7380581B2 (ja) | 二次電池およびその製造方法 | |
| US10714722B2 (en) | Composition for non-aqueous secondary battery functional layer, functional layer for non-aqueous secondary battery, and non-aqueous secondary battery | |
| US20240322374A1 (en) | Laminate for non-aqueous secondary battery, composition for adhesion, and non-aqueous secondary battery | |
| KR20190040192A (ko) | 비수계 이차 전지 다공막용 조성물, 비수계 이차 전지용 다공막 및 비수계 이차 전지 | |
| JP2017098203A (ja) | 非水系二次電池接着層用組成物、非水系二次電池用接着層、及び非水系二次電池 | |
| JP6515574B2 (ja) | 非水系二次電池機能層用バインダー、非水系二次電池機能層用組成物、非水系二次電池用機能層および非水系二次電池 | |
| JP7306271B2 (ja) | 非水系二次電池機能層用組成物、非水系二次電池用電池部材、非水系二次電池用積層体の製造方法、および、非水系二次電池 | |
| KR20190039932A (ko) | 비수계 이차 전지 기능층용 조성물, 비수계 이차 전지용 기능층 및 비수계 이차 전지 | |
| JP7732357B2 (ja) | 二次電池およびその製造方法 | |
| JP2017103031A (ja) | 非水系二次電池用積層体 | |
| WO2023189442A1 (ja) | 非水系二次電池機能層用スラリー組成物、非水系二次電池用セパレータ及び非水系二次電池 | |
| WO2019004460A1 (ja) | 電気化学素子用バインダー組成物、電気化学素子機能層用スラリー組成物、電気化学素子接着層用スラリー組成物、および複合膜 | |
| JP6665484B2 (ja) | 非水系二次電池接着層用組成物、非水系二次電池用接着層、及び非水系二次電池 | |
| WO2023032718A1 (ja) | 非水系二次電池接着層用組成物、非水系二次電池用接着層及びその製造方法、非水系二次電池用積層体及びその製造方法、並びに、非水系二次電池 | |
| WO2022209997A1 (ja) | 非水系二次電池接着層用組成物、非水系二次電池用接着層およびその製造方法、非水系二次電池用積層体およびその製造方法、ならびに、非水系二次電池 | |
| US20250129274A1 (en) | Composition for non-aqueous secondary battery adhesive layer, adhesive layer for non-aqueous secondary battery, battery member for non-aqueous secondary battery and method of producing same, laminate for non-aqueous secondary battery and method of producing same, and non-aqueous secondary battery | |
| WO2024135749A1 (ja) | 電気化学素子機能層用組成物、電気化学素子用部材、電気化学素子用積層体の製造方法、および電気化学素子 | |
| WO2023008165A1 (ja) | 非水系二次電池用積層体、非水系二次電池用積層体の製造方法及び非水系二次電池 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23759611 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202380015784.2 Country of ref document: CN |
|
| ENP | Entry into the national phase |
Ref document number: 2024502951 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 18835350 Country of ref document: US |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023759611 Country of ref document: EP |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| ENP | Entry into the national phase |
Ref document number: 2023759611 Country of ref document: EP Effective date: 20240930 |
|
| WWP | Wipo information: published in national office |
Ref document number: 18835350 Country of ref document: US |