WO2022158339A1 - Procédé d'impression à jet d'encre - Google Patents

Procédé d'impression à jet d'encre Download PDF

Info

Publication number
WO2022158339A1
WO2022158339A1 PCT/JP2022/000614 JP2022000614W WO2022158339A1 WO 2022158339 A1 WO2022158339 A1 WO 2022158339A1 JP 2022000614 W JP2022000614 W JP 2022000614W WO 2022158339 A1 WO2022158339 A1 WO 2022158339A1
Authority
WO
WIPO (PCT)
Prior art keywords
resin
ink
acid
recording method
pigment
Prior art date
Application number
PCT/JP2022/000614
Other languages
English (en)
Japanese (ja)
Inventor
学 金子
Original Assignee
コニカミノルタ株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by コニカミノルタ株式会社 filed Critical コニカミノルタ株式会社
Priority to JP2022576614A priority Critical patent/JPWO2022158339A1/ja
Publication of WO2022158339A1 publication Critical patent/WO2022158339A1/fr

Abstract

Ce procédé d'impression à jet d'encre comprend l'application d'un fluide de pré-revêtement sur une base, l'impression d'une encre à base d'eau simultanément avec cette dernière ou immédiatement après, et le séchage de l'encre à base d'eau, le fluide de pré-revêtement contenant un acide organique ou un sel de métal polyvalent et l'encre à base d'eau comprenant un pigment, une dispersion de fines particules de résine, de l'eau et un solvant organique, la dispersion de fines particules de résine satisfaisant l'exigence (I). Exigence (I) : un mélange liquide préparé par addition d'une solution aqueuse d'acide malonique à la dispersion de fines particules de résine de manière à obtenir une teneur en fines particules de résine de 5 % en masse et une concentration en acide malonique de 10 mmol/L présente un pH à 25 °C de 5 ou moins.
PCT/JP2022/000614 2021-01-21 2022-01-12 Procédé d'impression à jet d'encre WO2022158339A1 (fr)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2022576614A JPWO2022158339A1 (fr) 2021-01-21 2022-01-12

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021-007664 2021-01-21
JP2021007664 2021-01-21

Publications (1)

Publication Number Publication Date
WO2022158339A1 true WO2022158339A1 (fr) 2022-07-28

Family

ID=82549732

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/000614 WO2022158339A1 (fr) 2021-01-21 2022-01-12 Procédé d'impression à jet d'encre

Country Status (2)

Country Link
JP (1) JPWO2022158339A1 (fr)
WO (1) WO2022158339A1 (fr)

Citations (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2009030014A (ja) * 2007-06-25 2009-02-12 Riso Kagaku Corp 捺染インクジェット用インク
JP2017024365A (ja) * 2015-07-27 2017-02-02 富士フイルム株式会社 画像記録方法
JP2018184696A (ja) * 2018-06-15 2018-11-22 セイコーエプソン株式会社 インクジェット記録方法及び記録装置
JP2019162756A (ja) * 2018-03-19 2019-09-26 株式会社リコー 記録方法、及び記録装置
JP2020007543A (ja) * 2018-06-28 2020-01-16 理想科学工業株式会社 インクジェット捺染用インク及びインクセット
JP2020045382A (ja) * 2018-09-14 2020-03-26 マクセルホールディングス株式会社 インクジェット用インクセット、および、インクジェット記録方法
JP2020176218A (ja) * 2019-04-19 2020-10-29 サカタインクス株式会社 インクセット、印刷物、および画像形成方法
JP2020189897A (ja) * 2019-05-20 2020-11-26 コニカミノルタ株式会社 インクジェット記録液セット、画像形成方法および印刷物

Patent Citations (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2009030014A (ja) * 2007-06-25 2009-02-12 Riso Kagaku Corp 捺染インクジェット用インク
JP2017024365A (ja) * 2015-07-27 2017-02-02 富士フイルム株式会社 画像記録方法
JP2019162756A (ja) * 2018-03-19 2019-09-26 株式会社リコー 記録方法、及び記録装置
JP2018184696A (ja) * 2018-06-15 2018-11-22 セイコーエプソン株式会社 インクジェット記録方法及び記録装置
JP2020007543A (ja) * 2018-06-28 2020-01-16 理想科学工業株式会社 インクジェット捺染用インク及びインクセット
JP2020045382A (ja) * 2018-09-14 2020-03-26 マクセルホールディングス株式会社 インクジェット用インクセット、および、インクジェット記録方法
JP2020176218A (ja) * 2019-04-19 2020-10-29 サカタインクス株式会社 インクセット、印刷物、および画像形成方法
JP2020189897A (ja) * 2019-05-20 2020-11-26 コニカミノルタ株式会社 インクジェット記録液セット、画像形成方法および印刷物

Also Published As

Publication number Publication date
JPWO2022158339A1 (fr) 2022-07-28

Similar Documents

Publication Publication Date Title
EP3211048B1 (fr) Composition liquide de traitement de surface, ensemble d'encre, procédé d'enregistrement et dispositif d'enregistrement
JP7110755B2 (ja) インクジェット記録液セット、インクジェット記録用前処理液の製造方法、印刷物及びインクジェット記録方法
JP7091776B2 (ja) インクジェット記録用前処理液、インクジェット記録液セット、インクジェット記録用前処理液の製造方法、印刷物及びインクジェット記録方法
JP6821874B2 (ja) 積層体及びその製造方法
JP7516927B2 (ja) インクジェット記録液セットおよび当該インクジェット記録液セットを用いる画像形成方法
WO2021157310A1 (fr) Procédé d'impression à jet d'encre et article imprimé par image
WO2019044673A1 (fr) Procédé de formation d'image à jet d'encre
JP2023507767A (ja) インクジェットインク及びプライマー流体セット
JP7214984B2 (ja) インクジェット記録液セット及びインクジェット記録方法
JP7251308B2 (ja) インクジェット記録液セット、画像形成方法および印刷物
JP7192376B2 (ja) インクジェット記録液セット、インクジェット記録用前処理液の製造方法、印刷物及びインクジェット記録方法
JP6988915B2 (ja) インクジェット記録用前処理液、その製造方法、インクジェット記録液セット、印刷物及びインクジェット記録方法
JP7092150B2 (ja) 水性インクジェットインク、水性インクジェットインクの製造方法、印刷物及びインクジェット記録方法
WO2022219816A1 (fr) Ensemble d'encres et procédé d'impression à jet d'encre
WO2022158339A1 (fr) Procédé d'impression à jet d'encre
JP7180262B2 (ja) インクジェット記録用前処理液、インクジェット記録用前処理液の製造方法、インクジェット記録液セット、印刷物及びインクジェット記録方法
WO2023105737A1 (fr) Jeu d'encre pour impression à jet d'encre, procédé d'impression à jet d'encre et dispositif d'impression à jet d'encre
JP2023507643A (ja) インクジェットインクおよびプライマー流体セット
JP2023507768A (ja) インクジェットインクおよびプライマー流体セット
WO2022219815A1 (fr) Jeu d'encres et procédé d'impression à jet d'encre
WO2024195600A1 (fr) Ensemble d'encres, procédé d'enregistrement à jet d'encre et système d'enregistrement à jet d'encre
WO2023175818A1 (fr) Encre d'enregistrement à jet d'encre, procédé de fabrication d'encre d'enregistrement à jet d'encre, ensemble d'encres d'enregistrement à jet d'encre, procédé de formation d'image et dispositif de formation d'image
JP7528575B2 (ja) 前処理液、当該前処理液を含むインクジェット記録液セットおよび画像形成方法
WO2023176719A1 (fr) Procédé de formation d'image et dispositif de formation d'image
JP2023087706A (ja) インクセット及び画像形成方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22742461

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2022576614

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase