WO2020181244A1 - Rechargeable li-ion battery with halogen intercalated graphite electrode - Google Patents

Rechargeable li-ion battery with halogen intercalated graphite electrode Download PDF

Info

Publication number
WO2020181244A1
WO2020181244A1 PCT/US2020/021527 US2020021527W WO2020181244A1 WO 2020181244 A1 WO2020181244 A1 WO 2020181244A1 US 2020021527 W US2020021527 W US 2020021527W WO 2020181244 A1 WO2020181244 A1 WO 2020181244A1
Authority
WO
WIPO (PCT)
Prior art keywords
lithium
ion battery
graphite
rechargeable
battery according
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2020/021527
Other languages
English (en)
French (fr)
Inventor
Chunsheng Wang
Chongyin YANG
Jijian Xu
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of Maryland, College Park
Original Assignee
University of Maryland, College Park
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Maryland, College Park filed Critical University of Maryland, College Park
Priority to CN202080018985.4A priority Critical patent/CN113544878B/zh
Priority to EP20766129.9A priority patent/EP3935680A4/en
Priority to KR1020217031016A priority patent/KR102813666B1/ko
Priority to US17/436,609 priority patent/US12142722B2/en
Priority to CN202510730513.6A priority patent/CN120581728A/zh
Priority to KR1020257016994A priority patent/KR20250084228A/ko
Priority to JP2021552631A priority patent/JP7599221B2/ja
Publication of WO2020181244A1 publication Critical patent/WO2020181244A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/052—Li-accumulators
    • H01M10/0525—Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/36—Accumulators not provided for in groups H01M10/05-H01M10/34
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/056—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes
    • H01M10/0564—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes the electrolyte being constituted of organic materials only
    • H01M10/0565—Polymeric materials, e.g. gel-type or solid-type
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/056—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes
    • H01M10/0564—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes the electrolyte being constituted of organic materials only
    • H01M10/0566—Liquid materials
    • H01M10/0568—Liquid materials characterised by the solutes
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00—Secondary cells; Manufacture thereof
    • H01M10/05—Accumulators with non-aqueous electrolyte
    • H01M10/056—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes
    • H01M10/0564—Accumulators with non-aqueous electrolyte characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes the electrolyte being constituted of organic materials only
    • H01M10/0566—Liquid materials
    • H01M10/0569—Liquid materials characterised by the solvents
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/04—Processes of manufacture in general
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/04—Processes of manufacture in general
    • H01M4/043—Processes of manufacture in general involving compressing or compaction
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
    • H01M4/133—Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/13—Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
    • H01M4/139—Processes of manufacture
    • H01M4/1393—Processes of manufacture of electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/362—Composites
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/362—Composites
    • H01M4/364—Composites as mixtures
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/58—Selection of substances as active materials, active masses, active liquids of inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy; of polyanionic structures, e.g. phosphates, silicates or borates
    • H01M4/582—Halogenides
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/58—Selection of substances as active materials, active masses, active liquids of inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy; of polyanionic structures, e.g. phosphates, silicates or borates
    • H01M4/583—Carbonaceous material, e.g. graphite-intercalation compounds or CFx
    • H01M4/587—Carbonaceous material, e.g. graphite-intercalation compounds or CFx for inserting or intercalating light metals
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/36—Selection of substances as active materials, active masses, active liquids
    • H01M4/60—Selection of substances as active materials, active masses, active liquids of organic compounds
    • H01M4/602—Polymers
    • H01M4/604—Polymers containing aliphatic main chain polymers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/62—Selection of inactive substances as ingredients for active masses, e.g. binders, fillers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M4/00—Electrodes
    • H01M4/02—Electrodes composed of, or comprising, active material
    • H01M4/62—Selection of inactive substances as ingredients for active masses, e.g. binders, fillers
    • H01M4/621—Binders
    • H01M4/622—Binders being polymers
    • H01M4/623—Binders being polymers fluorinated polymers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M2300/00—Electrolytes
    • H01M2300/0017—Non-aqueous electrolytes
    • H01M2300/0025—Organic electrolyte
    • H01M2300/0028—Organic electrolyte characterised by the solvent
    • H01M2300/0037—Mixture of solvents
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01M—PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M2300/00—Electrolytes
    • H01M2300/0085—Immobilising or gelification of electrolyte
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E60/00—Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
    • Y02E60/10—Energy storage using batteries

Definitions

  • the present invention relates to rechargeable lithium ion batteries comprising a lithium salt-graphite composite electrode.
  • the present invention relates to a rechargeable“water-in-salt” lithium ion battery with a high potential where at least a portio of the lithium salt is phase separated from the aqueous electrolyte.
  • Lithium ion batteries are a useful and powerful energy storage option. Their use has been expanding to a variety of products including, but not limited to, portable electronics (e.g., computers, mobile phones, speakers, etc.) to hybrid and electric cars. Lithium ion batteries are low maintenance and display higher charge storage densities and voltages and out-perform typical lead-acid batteries, as the small lithium-ions can pack densely into the anode material.
  • Intercalation cathode chemistries used in state-of-the-art Li-ion batteries store electrical energy by accommodating Li + in their lattices with charge compensation from cationic redox reactions of transition metals (Ni, Co, Mn, Fe, etc.), which occurs with superior reversibility (long cycle life) but delivers mediocre capacities ( ⁇ 200 mAh g _1 ) due to their heavy molar mass per intercalated Li + and potential structural instability upon over-delithiation.
  • the anionic redox reactions (O/O 2 , S/S 2 , etc.), on the other hand, promise much higher capacities by following a conversion reaction mechanism, but normally proceed with extremely poor reversibility, which arises from the repeated breaking and re-formation of structures and the accompanied large volume change upon each charge/discharge cycle.
  • the low electronic and ionic conductivities of these anionic redox materials further worsen the issue.
  • intercalation host has been recently discovered in Li-excess transition metal oxide materials, where the oxygen layer participates the cell reaction and significantly contributed to the overall capacity of transition metal oxides.
  • Lithium batteries based on anionic-redox reaction that occurs in an intercalation host would be highly attractive, as it would inherit both the high energy of anionic-redox conversion-reaction and the excellent reversibility from topotactic mechanism of intercalation.
  • PF 6 -, BFL, TFSL anions in electrolyte of‘dual-ion’ batteries can be reversibly intercalated into graphite. However, these redox reactions only occur on graphite lattice rather than anion themselves, limiting the capacity below 120 mAh g 1 .
  • Redox of S/S n 2 and Br7Br 3 _ catholytes in porous carbon are highly reversible, but these anions were only physically confined in/adsorb on the porous carbon, resulting in high self-discharge and low cycle life due to undesired shuttling reaction.
  • the anion-catholytes should phase-separate from electrolytes, while oxidized anions should be stabilized via intercalation in a solid host.
  • no suitable anions, intercalation host and electrolytes have been identified to support this ideal energy storage mechanism with sufficient capacity at a high potential.
  • a rechargeable lithium-ion battery i.e., lithium battery
  • the lithium battery comprises: (i) a composite cathode comprising a lithium salt and graphite; (ii) an electrolyte; and (iii) an anode.
  • the composite cathode is configured such that the oxidation product of the lithium salt is or becomes intercalated in said graphite.
  • the lithium-ion battery has a capacity of greater than 200 mAh/g, typically at least about 230 mAh/g, often at least about 240 mAh/g, and most often at least about 250 mAh/g.
  • an energy density of said lithium-ion battery is at least about 400 Wh/kg, typically at least about 430 Wh/kg, often at least about 460 Wh/kg, and most often at least about 500 Wh/kg.
  • Such a value determination will depend at least in part on how the value is measured or determined, e.g., the limitations of the measurement system, i.e., the degree of precision required for a particular purpose.
  • the term“about” can mean within 1 or more than 1 standard deviation, per the practice in the art.
  • the term“about” when referring to a numerical value can mean ⁇ 20%, typically ⁇ 10%, often ⁇ 5% and more often ⁇
  • the coulombic efficiency of said lithium battery is at least about 95%, typically at least about 98 %, often at least about 99 %, and most often at least about 99.9 %.
  • said lithium-ion battery has a potential of at least about 4 V vs. Li/Li + , typically at least about 4.1 V, often at least about 4.15 V, and most often at least about 4.2 V.
  • the composite cathode comprises a plurality of lithium salts, such as lithium halide salts. Still in other embodiments, the composite cathode comprises lithium chloride, lithium bromide, lithium iodide, lithium fluoride, and other halogen salts or a combination thereof. In one particular embodiment, the composite cathode comprises a combination of lithium chloride and lithium bromide.
  • the electrolyte comprises a fluoride-based electrolyte.
  • Exemplary fluoride-based electrolytes that can be used in lithium batteries of the invention include, but are not limited to, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiOTf), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium difluoro(oxalato)b orate (LiDFOB), lithium hexafluoroarsenate (Li AsFr > ), Lithium perchlorate (LiClCE), Lithium nitrate (L1NO 3 ) or electrolytes that can be phase-separated with lithium halogen salt electrolyte and a mixture thereof.
  • LiTFSI lithium bis(trifluoromethanesulfonyl)imide
  • LiOTf lithium triflu
  • said electrolyte comprises water-in-bisalt electrolyte
  • LiBS Li-Silicate
  • a highly concentrated organic electrolyte an all-solid-state ceramic electrolyte, an electrolyte that can phase separate with lithium halogen salt electrolyte, or a combination thereof.
  • Exemplary highly concentrated organic electrolytes include, but are not limited to,
  • LiTFSI lithium bis(trifluoromethanesulfonyl)imide
  • LiDFOB lithium difluoro(oxalato)borate
  • L1BF4 lithium tetrafluoroborate
  • EC ethylene carbonate
  • LiFSI lithium bis(fluorosulfonyl)imide
  • FEC fluoroethylene carbonate
  • L1BF4 2m lithium tetrafluoroborate
  • Exemplary all-solid-state ceramic electrolytes include, but are not limited to,
  • said electrolyte is in a form of an aqueous gel.
  • said electrolyte further comprises poly(ethylene oxide), polyvinyl alcohol, polyacrylonitrile, poly(methyl methacrylate), polyacrylic acid, polytetrahydrofuran, polyethylene glycol dimethacrylate, poly(ethylene glycol) diacrylate, 2-hydroxyethyl acrylate, poly(ethylene glycol) methyl ether, bisphenol A ethoxylate dimethacrylate, polyvinylpyrrolidone and other hydrophilic polymers, or a combination thereof.
  • Another aspect of the invention provides a method for producing a lithium salt- graphite composite cathode for use in a rechargeable lithium ion battery.
  • the lithium salt is intercalated in said graphite.
  • the method includes compressing a mixture of a lithium salt-graphite composite material and a polymer under conditions sufficient to produce a lithium salt graphite composite cathode, whereby an oxidation of the lithium salt results in intercalation of an oxidation product of the lithium salt within the graphite.
  • the method further comprises the steps of admixing a lithium salt and graphite and milling said mixture to produce said lithium salt-graphite composite material prior to admixing with said polymer.
  • the lithium salt comprises two or more lithium salts, typically lithium halide salts.
  • the lithium salt is a mixture of lithium bromide and lithium chloride.
  • the molar ratio of lithium bromide to lithium chloride is about 5 : 1, typically about 3 : 1, often about 2 : 1, and most often about 1 : 1.
  • the mass ratio of said lithium bromide, said lithium chloride, and said graphite is about 2: 0.25 : 2, typically about 2 : 0.5 : 2, and often about 2: 1 :2.
  • said polymer comprises poly(vinylidenedifluoride)
  • PTFE polyvinylidene difluoride
  • PVDF polyvinylidene difluoride
  • PVP polyvinylpyrrolidone
  • SBR styrene-butadiene rubber
  • CMC carboxymethyl cellulose
  • alginic acid l,l,2,2-tetrafluoroethyl-2,2,2- trifluoroethyl ether, l,l,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2- trifluoroethyl) ether, or a mixture thereof.
  • said polymer comprises PTFE.
  • the mass ratio of said lithium salt-graphite composite material to said polymer is about 90 : 10, typically about 92 : 8, often about 94 : 6, and most often about 95:5.
  • Yet another aspect of the invention provides a rechargeable lithium-ion battery comprising: (i) a composite cathode comprising at least one lithium salt and graphite, wherein the composite cathode is configured such that an oxidation of the lithium salt results in intercalation of an oxidation product of the lithium salt within the graphite; (ii) an aqueous electrolyte; and (iii) an anode comprising a fluorinated polymer.
  • said aqueous electrolyte comprises water-in-bisalt electrolyte (WiBS).
  • said WiBS comprises lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiOTf), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF 6 ), Lithium
  • LiDFOB Lithium difluoro(oxalato)borate
  • Li AsFr > Li AsFr >
  • Me3EtN TFSI asymmetric ammonium salt
  • pyrl3TFSI N-propyl-N- methylpyrrolidinium bis(trifluoromethanesulfonyl)imide
  • other ionic liquid or a mixture thereof.
  • WiBS may also include organic solvent.
  • organic solvents include, but are not limited to, trimethyl phosphate, ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), propylene carbonate (PC), g-butyrolactone (y-BL), ethyl methyl carbonate, dimethoxyethane, diglycol methyl ether, fluoroethylene carbonate (FEC) and derivatives thereof, as well as other organic solvents that are known to one skilled in the art or used in lithium-ion batteries. See, for example, Long et al., in“Polymer electrolytes for lithium polymer batteries,” J. Mater. Chem. A , 2016, 4, pp.
  • the amount of organic solvent used relative to water is about 66% or less (i.e., 2 or less : 1) by volume, typically about 50% or less (i.e., 1 or less : 1) by volume, and often about 20% or less (i.e., 1 or less : 4) by volume.
  • At least a portion of said lithium salt is phase-separated from said aqueous electrolyte.
  • the anode is protected by said fluorinated polymer.
  • said fluorinated polymer is a fluorinated ether polymer.
  • said fluorinated polymer comprises a highly fluorinated ether (HFE) polymer gel (such as l,l,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, l,l,2,2-tetrafluoroethyl-2,2,3,3- tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, or a mixture thereof.
  • HFE highly fluorinated ether
  • Figure 1 is a schematic illustration of the conversion-intercalation mechanism occurring in LBC-G composite during its oxidation in WiBS aqueous-gel electrolyte.
  • the two- stage reactions involved the oxidation of Br ( ⁇ 4.0 V) and CL ( ⁇ 4.2 V) and their subsequent intercalation into graphitic structure.
  • the discharge was a complete reversal of the charge process.
  • Figure 2 is a cyclic voltammogram of LBC-G cathode between 3.2 and 4.9 V vs.
  • Li/Li + at scan rate of 0.05 mVs 1 Li/Li + at scan rate of 0.05 mVs 1 .
  • Figure 3 is a galvanostatic charge/discharge profiles of LBC-G cathode at a current density of 80 mA g 1 . Insert: Discharge capacity retention and coulombic efficiencies.
  • Figure 4 is a linear sweep voltammetry of pure graphite electrode (with only
  • PTFE binder on Ti mesh current collector in LiBreFLO, LiClGFLO, and WiBS electrolyte with Ag/AgCl electrode as reference at 1 mV/s, showing absence of side reactions including corrosion of the current collector and oxidations of graphite and water before the onsets at ⁇ 4.0 V, 4.5 V and 5.0 V vs. Li/Li+, in according with the oxidations of Br-, C1-, and water, respectively.
  • Figure 5 is a graph of GITT characterization of LBC-G cathode at a current density of 80 mA g 1 .
  • Red curve is quasi-equilibrium potential at different lithiation/de-lithiation stages, which was constructed from the average value of each open-circuit voltage period during charge/discharge.
  • Inset The finite diffusion coefficients D of reactants estimated from GITT and EIS measurements.
  • Figure 6 is a Nyquist plots for LBC-G cathode obtained by EIS tests at various
  • Figure 7 is In situ Raman spectra (100 - 550 cm 1 ) of LBC-G during the entire charge-discharge cycle, showing the evolutions of Br2 and BrCl intercalants.
  • Red line Free BrCl signals detected only after deliberately destabilizing the graphite host with a strong laser beam, further confirming the BrCl intercalation. Background from quartz was removed.
  • Figure 8 (2b) is an ex situ Br K-edge XANES of LBC-G composite during its first charging process. Chemically intercalated Br2 and liquid Br2 as control samples (dash curves) were measured in the same cell configuration.
  • Figure 9 (2c) is an ex situ Cl K-edge XANES of LBC-G composite during its first charging process.
  • Figure 10 illustrates the charge/discharge profiles of LBC-G composites with various mole ratios of LiBr/LiCl after the first charge at the current density of 80 mA g 1 . The specific capacities were estimated by the weight of LiBr and LiCl. The mole ratios were changed by only reducing the certain portions of LiCl from the original LiBr/LiCl/graphite composites.
  • Figure 11 (2f) illustrates the charge/discharge profiles of LBC-G composites with various mole ratios of LiBr/LiCl after the first charge at the current density of 80 mA g 1 .
  • the specific capacities were estimated by the weight of LiBr and LiCl.
  • the mole ratios were changed by only reducing the certain portions of LiBr from the original LiBr/LiCl/graphite composites.
  • Figure 12 (3a) is an in situ Raman spectra (1200 - 2850 cm 1 ) of LBC-G during the entire charge-discharge cycle, showing the graphite structure evolution with Br2 and BrCl intercal ati on/ de-intercal ati on .
  • Figure 13 (3b) is an ex situ XRD of LBC-G composite in various charging and discharging states through the second cycle.
  • Q-2Q scan mode was employed with Cu K a radiation (1.5418 A) in reflection geometry.
  • Left overall spectra.
  • Middle magnified range of 2Q (24°-28°).
  • Right magnified range of 2(9(48°-60°) The peaks of titanium current collectors were used to calibrate the diffraction angles.
  • Figure 14 (3c) is an in situ XRD patterns of ( 0 0 m+1 ) peak for LBC-G composite during a charge-discharge cycle, which were collected with high-energy X-ray radiation (wavelength of 0.1173 A) in transmission geometry.
  • Left Corresponding voltage profile.
  • Right 2D contour of XRD patterns and representative curves illustrating the continuous evolution of d spacing (3.30-3.55 A) for graphite host during intercalation/de-intercalation. The 2 Q diffraction angles were converted to d spacing for convenience (see Methods).
  • Figure 15 (3d) is an ex situ High-energy XRD patterns for LBC-G composites
  • Figures 16 A and 16B are the best-fit modes for Br EXAFS experimental data of
  • the EXAFS spectra here in R Space are phase-uncorrected, so that the distance R in two Figures for two stages are not comparable but both are smaller than the actual values.
  • Inset In-plane configurations of Stage II C ? [Br] and Stage I C3 . 5[Bro . 5Clo . 5] obtained from DFT simulations. Two sets of bond distances were marked as red lines (short) and blue lines (long).
  • Figure 17 (4a) is a graph showing a typical charge-discharge voltage profiles (the
  • LBC-G cathodes consisting of anhydrous LiBr/LiCl (blue) or LiBr/LiCl monohydrates (red) and HFE/PEO protected graphite anodes. Charging and discharging were performed at 0.2 C (44 mA g 1 for LBC-G cathode) at 25 °C. The cell capacity was calculated on the basis of the cathode mass alone (upper X-axis) or the total mass of cathode and anode including binder and protective coating (bottom x-axis).
  • Figure 18 (4b) is a graph showing the discharge capacities (on total mass of cathode and anode, open circles) and coulombic efficiencies (semi-solid circles) of full cells during cycling in one particular embodiment of lithium-ion battery of the invention.
  • Figure 19 (4c) shows discharge capacities calculated on total anode and cathode mass at various rates of one particular embodiment of LBC-G/graphite full cells of the invention with different electrolyte/electrodes (cathode + anode) mass ratios.
  • Figure 20 shows a galvanostatic charge/discharge profiles of LBC-G cathode in
  • Figure 21 shows a galvanostatic charge/discharge profiles of LBC-G cathode in
  • lithium batteries with a capacity of at least about 200 mAh/g, typically at least about 210 mAh/g, often at least about 220 mAh/g, more often at least about 230 mAh/g, and most often at least about 240 mAh/g (of total weight of composite electrode).
  • lithium batteries having an average potential of at least about 4.0 V, typically at least about 4.1 V, and often at least about 4.2 V (versus Li/Li +).
  • Such a high capacity and/or high potential lithium battery is possible due to the discovery by the present inventors of a new electrode that intercalates a lithium salt within the graphite. Without being bound by any theory, it is believed that in lithium batteries of the invention the anionic-redox reaction occurs within the graphite lattice and the oxidized anions are stabilized by intercalation into graphite lattice, thereby avoiding the problems associated with conventional batteries utilizing intercalation cathode chemistry.
  • Intercalation cathode chemistries used in Li-ion batteries store electrical energy by accommodating Li + in their lattices with charge compensation from cationic redox reactions of transition metals (e.g., Ni, Co, Mn, Fe, etc.), which occurs with superior reversibility (long cycle life) but delivers a relatively low capacities due to their heavy molar mass per intercalated Li + and potential structural instability upon over-delithiation.
  • transition metals e.g., Ni, Co, Mn, Fe, etc.
  • lithium-ion batteries of the invention include a water-in- bisalt (WiBS) electrolyte. It is believed that the WiBS electrolyte enables or enhances a conversion-intercalation reaction.
  • the conversion reaction refers to anionic oxidation reaction, for example, conversion of bromide ion to bromine gas or conversion of chloride ion to chlorine gas, or conversion of a mixture of bromide and chloride ions to bromine gas, chlorine gas, and/or Br-Cl gas.
  • Some aspects of the invention are based on the anionic-redox reaction of halide anions (Br and CL).
  • halide anions Br and CL
  • both the anionic-redox reaction of halide anions and the resulting oxidation products remain intercalated or entrapped within the electrode, e.g., graphite, lattice.
  • a composite electrode containing graphite with equimolar lithium halide salts ((LiBr)o . 5(LiCl)o . 5-graphite, hereafter denoted as LBC-G) was prepared as active material.
  • WiBS electrolye is used in lithium batteries of the invention.
  • the highly concentrated WiBS electrolyte confines at least a portion of the hydrated LiBr and LiCl inside the solid cathode matrix.
  • the anionic-redox reaction i.e., oxidation of bromide and chloride anions, to the oxidized products, e.g., Br° and Cl°, is believed to occur within the graphite lattice and the oxidized products are stabilized by their intercalation into graphitic structure.
  • lithium-ion batteries that utilize high density halide ion packing and a water-in-salt electrolyte to achieve a potential of over 4 volts in aqueous batteries. It is believed that lithium salts within the graphite lattice are phase-separated from aqueous electrolytes. Accordingly, other aspects of the invention provide a rechargeable lithium-ion battery having at least a portion of lithium salt that is phase-separated from an aqueous electrolyte.
  • life cycle when referring to a battery is defined as a total number of recharging while still maintaining coulombic efficiency of at least 99%, typically at least 99.5%, and often at least 99.9%.
  • the term“life cycle” refers to the number of total cycle that the battery can be recharged before having its capacity drop or fall below about 80%, typically about 85%, and often about 90% of its theoretical capacity.
  • the term“cycle” when referring to a battery means a recharging of the battery, typically recharging from about 5% or less charge to at least about 90% charge.
  • the“life cycle” of a battery by allowing the battery’s charge to deplete to about 5% or less of the theoretical charge and recharging the battery to at least about 90% of the theoretical charge, and repeating the process until either the coulombic efficiency or the capacity of the battery falls below the amount as defined herein.
  • the lithium batteries of the invention have capacity retention of at least about 70%, typically at least about 75%, often at least about 80%, more often at least about 85%, and most often at least about 90% after 100 cycles.
  • the lithium battery of the invention has capacity retention of at least about 80%, typically at least about 85%, often at least about 90%, and more often at least about 95% after 100 cycles.
  • the lithium battery of the invention has coulombic efficiency of at least about 80%, typically at least about 85%, often at least about 90%, more often at least 95%, and most often at least about 98% throughout its life cycle. Still in other embodiments, the lithium battery of the invention has coulombic efficiency of at least 99%, typically at least 99.5%, and often at least 99.9% throughout its life cycle.
  • the lithium battery of the invention has energy density of at least about 250 Wh kg 1 , typically at least about 300 Wh kg 1 , often at least about 350 Wh kg 1 , more often at least about 400 Wh kg 1 , and most often at least about 450 Wh kg 1 . It should be appreciated that the scope of the invention is not limited to these particular energy densities. In fact, the energy density of a particular battery of the invention depends on a variety of factors such as, but not limited to, the lithium salt(s), the anode material, the aqueous electrolyte, etc.
  • the theoretical energy capacity was calculated to be 309 mAh g _1 and 632 mAh g _1 , respectively, at a high delithiation/lithiation potentials of 4.0 - 4.5 V vs. Li/Li + .
  • These values for the theoretical energy capacity and the potential are significantly higher than those of other anions, e.g., sulfur at ⁇ 2.2 V or oxygen at ⁇ 3.0 V.
  • the reversible redox reaction of these halide anions followed by their intercalation into graphite creates a densely- loaded stage I intercalation compound C3 . 5[Bro . 5Clo .
  • the highly concentrated WiBS electrolyte confined the partially hydrated LiBr and LiCl inside the solid cathode matrix, while upon oxidation, Br° and Cl° are stabilized by their intercalation into graphitic structure, providing theoretical capacities of 309 mAh g _1 for LiBr and 632 mAh g _1 for LiCl at a high
  • delithiation/lithiation potentials of 4.0 - 4.5 V vs. Li/Li + , which are higher than those of sulfur at ⁇ 2.2 V or oxygen at ⁇ 3.0 V.
  • the reversible redox reaction of these halide anions followed by their intercalation into graphite creates a densely-loaded stage I intercalation compound
  • This conversion-intercalation LBC-G chemistry distinctly differs from all graphite-intercalation chemistries by anions such as PF6-, BFU, TFSL in at least two aspects: Firstly, LBC-G cathode stores anions source (Br and CL) in highly dense solid state rather than in dilute liquid electrolyte. Therefore, the capacity is not restricted by salt solubility or electrolyte amount in principle. Secondly, during charge, the oxidized species in LBC-G are the
  • the halogen intercalation into graphite in LBC-G is also much faster and more reversible than crystal reconstruction reaction in transition metal halides, which is always accompanied with large kinetics hysteresis, massive volume changes and irreversible particle disintegration.
  • anion redox couples S/S n 2 , O/O 2 , Bn /Br , etc.
  • the dissolution of the intermedia also improved reaction kinetics
  • the final charging products are normally deposited or adsorbed on high surface area carbon host, leading to side reactions, parasitic shuttling effect and low volumetric energy densities.
  • Using super-concentrated WiBS electrolyte allows halide anions in hydration layer that is thermodynamically immiscible with WiBS to be confined within the cathode solid composite during repeated cycling of LBC-G, while the highly reactive oxidation product (BrCl, gaseous at room temperature) is effectively stabilized by its intercalation in graphite, thereby ensuring the high reversibility of this conversion-intercalation chemistry.
  • LBC-G composite cathode was prepared by mixing anhydrous LiBr and LiCl with graphite powder at a mass ratio of 2: 1:2 (corresponding to molar ratio of (LiBr)o . 5(LiCl)o . 5C3 . 7).
  • LBC-G composite cathode The electrochemical behavior of LBC-G composite cathode was evaluated in a three-electrode cell using active carbon (about 50 times the mass of the working electrode) as a counter electrode, Ag/AgCl as a reference electrode, and an aqueous gel polymer of 80 wt.% WiBS (21 mol kg 1 lithium bis(trifluorom ethane sulfonyl)imide (LiTFSI) - 7 mol kg 1 lithium
  • LiOTf trifluoromethane sulfonate
  • PEO polyethylene oxide
  • the anhydrous LiBr-LiCl salts in LBC-G extract trace water (approximate 2.4%) from WiBS, forming a hydrated LiBr-LiCl layer on the surface of LBC-G (estimated overall formulations of hydrated salts of LiBr 0.34H 2 0-LiC1 0.34H 2 0), which accelerate the redox reaction of halogens in the form of solvated anions.
  • this hydrated salt layer is
  • a liquefied layer allows for Li + transport but blocks the diffusion and potential undesired shuttling of halide ions, as evidenced by MD simulation as well as the extreme low Cl and Br content ( ⁇ 32 ppm) detected by chromatographic analysis in a WiBS electrolyte that has been equilibrated with LiCl-LiBr solution for 500 hours.
  • LBC-G indicated two distinct reactions at 4.0-4.2 V vs. Li/Li + for Br intercalation and 4.2-4.5 V vs. Li/Li + for Cl intercalation, respectively, which delivers a highly reversible discharge capacity of 243 mAh g _1 (of the total mass of LBC-G composite including LiBr/LiCl salts and graphite), 82% of which is retained over 230 cycles at a coulombic efficiency of 100 % after the 80 th cycle at a current density of 80 mA g _1 (0.2 C).
  • the two-step redox reactions correspond to:
  • Galvanostatic intermittent titration technique was used to examine the quasi-equilibrium potentials and kinetics of reactions at different stages.
  • the quasi-equilibrium potentials are -4.05 V for Br and -4.35 V for CT oxidation/intercalation reactions, respectively ( Figure 5), while the total diffusion coefficients were estimated in a range of 10 15 - 10 13 cm 2 s 1 (red and blue curves in the insert of Figure 5).
  • the diffusion coefficients of LBC-G cathodes were also investigated using electrochemical impedance spectroscopy (EIS), where Nyquist plots ( Figure 6) displayed two semicircles with the characteristic frequencies of - 1,250 Hz and - 20 Hz, respectively.
  • EIS electrochemical impedance spectroscopy
  • the semicircle at the high frequency range is attributed to the charge transfer resistance on the surface of graphite matrix, while the semicircle at a middle frequency range corresponds to salt dissolution/precipitation and finite diffusion of reactants in hydrated layer, and the slant-tail at a low frequency range is due to the halogen diffusion in graphite.
  • the apparent ionic diffusion coefficients (including dissolution/precipitation) of reactants was estimated to be 6.85 x 10 15 - 2.07 x 10 14 cm 2 s 1 (green circles in the insert of Figure 5), in excellent agreement with the estimated total diffusivity values from GITT measurements.
  • the mass transfer of Br and CL between solid salts and graphite surface constitutes the rate-determining step in this chemistry, which was also proved by their finite diffusion behavior.
  • LBC-G provides a practical gravimetric capacity of 231 mAh g _1 (of total weight of electrode), volumetric capacity of 450 mAh mL 1 (of total volume of electrode) at an average discharge voltage of 4.2 V vs. Li/Li + , yielding an extremely high energy density of 970 Wh kg -1 , which is almost twice as much as Ni-, Co-, and Mn-based intercalation cathode materials, or comparable with sulfur conversion cathode.
  • the volumetric energy density of LBC-G is much higher than that of sulfur. With both high gravimetric and volumetric energy densities, the conversion-intercalation nature of LBC-G makes it one of the most useful cathode chemistry for the lithium-ion batteries.
  • Carbon host can improve the reversibility and discharge capacity by surface adsorption of halogens, while the coulombic efficiency further increases with their graphitization degree. It is believed that the graphite intercalation provides reversible and compact manner to accommodate the oxidation products of halogens.
  • X-ray diffraction (XRD) spectra revealed a detailed evolution of the staging structure for LBC-G cathode.
  • Ex situ XRD of LBC-G cathodes showed shifting dominated peak of ( 0 0 m+1 ) and subdominant peak of ( 0 0 2m+2 ) during halogen intercalation/de-intercalation, further confirming the reference patterns.
  • Close examinations suggested a successive progression of d spacing for the dominated peak from 3.35 A for pristine graphite ( 0 0 2), to do 03 -3.45 A for stage II Br2 GIC when the SOC of LBC-G increases from 0% to 50%.
  • the in-plane configuration and coordination of halogen intercalants in GICs provide a method for determining the optimum intercalation concentration of LBC-G cathode chemistry. Since the in-plane intercalate structure was independent of intercalate concentration, the stoichiometry n of C n [Br] and C n [BrCl] always remain the same in each intercalation domain, regardless of the overall intercalation concentrations.
  • Aqueous LIB full cells were constructed by using an aqueous gel electrolyte derived from WiBS and coupling LBC-G cathode with a graphite anode that is protected by a highly fluorinated ether (HFE) polymer gel.
  • HFE highly fluorinated ether
  • the mass ratio of WiSB electrolyte to cathode may affect the rate performance of LBC-G cathodes. As shown in the upper part of Figure 19, the rate capability was compromised when the electrolyte/electrodes (cathode + anode) mass ratio was reduced from 4: 1 to 1 :2. Thus, in some embodiments, the
  • electrolyte/electrodes ratio is about 1 : 1, typically about 2 : 1, and often about 4 : 1.
  • high ratio of electrolyte to electrode will reduce the energy density.
  • LiBr and LiCl monohydrates LiBr tLO and LiCTFFO
  • LBC-G cathode with monohydrates showed almost identical charge/discharge profiles as the anhydrous one at low rate of 0.2C except for a slightly lower specific capacity ( Figures 17 and 18), which is due to the additional water mass brought by these monohydrates.
  • LiBr-H 2 0-LiCl H 2 0-G//G full cell is much higher than its anhydrous counterpart, while the impact of electrolyte/electrodes mass ratio is minimized. Since the battery performances constructed with LiBr-LiCl monohydrates are independent of electrolyte amount, it is estimated that the energy density of such aqueous LIBs to be around 460 Wh kg 1 of the total mass of cathode (with monohydrates) and anode. Such an energy density has never been reported for any known aqueous batteries, and are even higher than all the known state-of-the-art non-aqueous LIBs.
  • Non-aqueous LIB coin cells were constructed by using high concentration organic electrolyte and coupling LBC-G cathode with a lithium anode.
  • a high discharge capacity of 151 mAh/g (based on cathode mass) was obtained at a current density of 80 mA g 1 ( Figure 20).
  • the two-stage reactions involved the oxidation of Br 1 ( ⁇ 3.6 V) and CT 1 (-3.8 V) and their subsequent intercalation into graphitic structure.
  • the discharge capacity decreased to 83 mAh/g, corresponding to an initial coulombic efficiency of 55%.
  • the steady decay is mainly attributed to the Br2 dissolution.
  • the Br2 dissolution can be effectively prevented, showing more stable charge and discharge performance (Figure 21).
  • LiBr/LiCl/active carbon - 2 1 :9 for (LiBr)o . 5(LiCl)o . 5-AC; LiBr/LiCl/graphited acetylene black - 2: 1 :9 for (LiBr)o . 5(LiCl)o . 5-CB).
  • Composite LBC-G cathodes were fabricated by compressing LBC-G composite and poly(vinylidenedifluoride) (PTFE) at a weight ratio of 95:5 on a titanium metal mesh (Alfa Aesar, 100 mesh). The areal loading of cathode material was -38 mg cm 2 . The thickness of cathode is -200 pm.
  • Graphite anodes were fabricated by using synthetic graphite powder (TIMCAL TIMREX® KS44, particle size - 45.4 pm) and poly(vinylidenedifluoride) (PTFE) at a weight ratio of 9: 1 on a stainless steel mesh (200 mesh).
  • synthetic graphite powder TIMCAL TIMREX® KS44, particle size - 45.4 pm
  • PTFE poly(vinylidenedifluoride)
  • the liquid“water-in-bisalt” (WiBS) aqueous electrolytes were firstly prepared by dissolving 21 mol kg 1 LiTFSI (98%, TCI Co., Ltd.) and 7 mol kg 1 LiOTf (99.996%, Sigma-Aldrich) in water (HPLC grade).
  • Aqueous gel electrolytes were prepared by mixing 20 wt.% poly(ethylene oxide) (PEO, average M v ⁇ 600,000, Sigma- Aldrich) with WiBS electrolyte and heated at 80°C for 1 h in sealed glass molds. After cooling to the room temperature, sticky semi-solid WiBS gel electrolytes were obtained, which can be changed into any shape at 50 °C.
  • Br2 and BrCl GICs were prepared by exposing the graphite flasks (TIMCAL TIMREX ® KS4) in high-contraction Br2 (99.99%, Sigma-Aldrich) vapor and BrCl gas in well-sealed flasks for 2 hours.
  • BrCl was prepared by mixing the Br2 with equimolar of CE at -70 °C, which obtained by the reaction of trichloroisocyanuric acid and hydrochloric acid.
  • V m is the molar volume of partially hydrated LiBr/LiCl
  • F is the Faraday constant (96,486 C mol -1 )
  • S is the contact area between electrolyte and active materials
  • dE/dx is the slope of the coulometric titration curve at composition x
  • dE/dt I/2 can be obtained from the plot of the transient voltage versus the square root of time during constant current pulse.
  • the four-point EIS measurement was performed with Gamary 345 interface 1000 using 5 mV perturbation with the desired frequency range.
  • the full cells were assembled as a CR2032-type coin cell using LBC-G as cathode, and either sulfur-carbon or graphite electrodes as the anodes.
  • the cathode/anode mass ratios were set at 1.38: 1 for graphite anode cell.
  • a titanium metal foil disk was applied between cathode and coin cell case to prevent corrosion.
  • WiBS gel electrolyte was press into films and applied in the coin cells as both electrolyte and separator.
  • the mass ratio of total electrodes vs. electrolyte was in the range from 1 :4 to 2: 1.
  • the cell was heated to 50 °C for GPE self-healing.
  • the full cells were then cycled galvanostatically on a Land BT2000 battery test system (Wuhan, China) at room temperature.
  • m cathode was the total mass of cathode, including LiBr, LiCl, graphite and PTFE binder.
  • m anode was the total mass of anode, including graphite, PTFE binder and the polymer passivation coating.
  • High-energy synchrotron XRD measurements were carried out at the 11-ID-C beamline of the Advanced Photon Source (APS), Argonne National Laboratory.
  • a high-energy X-ray with beam size of 0.2 mmx0.2 mm and wavelength of 0.1173 A was used to obtain two-dimensional (2D) diffraction patterns in the transmission geometry.
  • X- ray patterns were recorded with a Perkin-Elmer large-area detector placed at 1800 mm from the battery cells. The interval between the consequent diffraction patterns was 5 min.
  • the obtained 2D diffraction patterns were calibrated using a standard CeCk sample and converted to ID patterns using Fit2D software.
  • the periodic repeat distance (/c), the intercalant gallery height (di) of GICs can be calculated using the following equation:
  • / is the index of (0 0 G) planes oriented in the stacking direction
  • d ots is the observed value of the spacing between two adjacent planes in XRD patterns, which can be calculated from diffraction angles by Bragg’s law.
  • the d spacing of pristine graphite is 3.35 A.
  • the intensity pattern is commonly found for a stage m graphite intercalation compound (GIC), where the most dominant peak is the (0 0 m+ 1).
  • GIC stage m graphite intercalation compound
  • the d spacing values of (0 0 m+ 1) were calculated from XRD data by Bragg's law, while the most dominant stage phase of the observed GIC can be assigned.
  • Eo is the absorption edge energy.
  • the theoretical calculated * h (k) is given by EXAFS equation:
  • N / is the coordination number of the shell
  • / / is the backscattering amplitude
  • R j is the average distance
  • s mean square variation
  • d is the scattering phase shift
  • l is the effective mean free path and s
  • j is the amplitude reduction factor
  • FEFF6 was used to calculate Jj, d, and l. Fitting to the experimental data to refine structure parameters ⁇ 2 , N j , R j , s 2 is done using Artemis program. The initial crystal structures for fitting are starting from DFT optimized Stage II C ? [Br] and Stage I C3 . 5[Bro . 5Clo 5]. S Q was fixed at 1.0. Two AE were used in the fitting, one for the Br-Br (or Cl) paths, and the other one for the left Br- C paths.
  • the 18m LiBr in H2O simulation cell contained 448 LiBr and 1390 H2O molecules.
  • the mixed salt MD simulation cell contained 1380 H2O, 512 LiTFSI and 448 LiBr. All simulated (LiTFSI) n (LiBr) m (H 2 0) k complexes resulting in large simulation cells of 70 and 95 A.
  • the simulation box dimensions were gradually decreased to 60 A.
  • NPT simulations were performed for 2 ns at 363 K for the mixed salt system at 363 K using a modified force field with the increased repulsion between Br/Br and TFSI/TFSI anions in order to evenly disperse them through the simulations box.
  • Multiple timestep integration was employed with an inner timestep of 0.5 fs (bonded interactions); a central time step of 1.5 fs for all nonbonded interactions within a truncation distance of 7.0-8.0 A and an outer timestep of 3.0 fs for all nonbonded interactions between 7.0 A and the nonbonded truncation distance of the smaller of 19 A.
  • the reciprocal part of Ewald was updated only at the largest of the multiple time steps.
  • a Nose-Hoover thermostat and a barostat were used to control the temperature and pressure with the associated frequencies of 10 2 and 0.1 x 10 4 fs.
  • the atomic coordinates were saved every 2 ps for post-analysis.
  • Ionic conductivity was extracted using the Einstein relations shown in the following equation: where e is the electron charge, Vis the volume of the simulation box, fe is Boltzmann’s constant, T is the temperature, t is time, zi and j are the Li + and Br charges, Ri(t) is the displacement of the ion i during time t, ⁇ > denote the ensemble average and N is the number of diffusing. Due to the finite size of the simulation cell, long range hydrodynamic interactions restrict diffusion. The leading order finite size correction (FSC) to the self-diffusion coefficient is given by the following equation:
  • the Br and Cl atoms were initialized randomly.
  • the geometry optimizations were performed using the conjugated gradient method, and the convergence threshold is set to be 10 5 eV in energy and 0.01 eV/A in force.
  • the charge difference plots were obtained by subtracting the charge density of both graphite and Br (BrCl) from the charge density of C ? [Br] (C3 . 5[Bro . 5Clo . 5]), respectively.
  • the charge distribution on the atoms were determined using the Bader analysis method. Visualization of the structures were made using VESTA software.
  • Intercalation voltage step profile simulation Intercalation voltage profiles were computed with CP2K v5.1 using the dispersion corrected (D3) PBE functional and double-z (triple-z for bromide) short-range, molecularly optimized valence basis sets and appropriate Goedecker-Teter-Hutter (GTH) pseudopotentials for core electrons.
  • the plane wave energy cutoff was set to 1000 Ry and the Brillouin zone was sampled at the G point only.
  • Geometry and cell optimizations were converged to a max change in atomic positions between steps of 0.0005 au. The other convergence criteria were left at their defaults.
  • the intercalation voltage (Emt) against Li + /Li can be computed from a series of energy calculations, assuming a negligible entropic contribution, as:
  • n x is the number of anions
  • E(GrX) is the energy of the intercalated graphite gallery
  • E(Gr) is the energy of pure graphite in AB-stacking
  • Edesoiv(LiX) is the desolvation energy of a LiX contact ion pair using the cluster-continuum method (with up to 8 explicit waters) from Gaussian calculations with PBEPBE+D3/6-3 lG(d)
  • Eg as (LiX) is the energy of the LiX contact ion pair in a 10 A x 10 A x 10 A cell
  • E b (Li) is the energy per Li in bulk metal (-204.1894 eV/Li).
  • 12 layers of carbon were modeled. Stage V was modeled with 10 layers of carbon. Each layer consisted of 112 carbon atoms.

Landscapes

  • Chemical & Material Sciences (AREA)
  • General Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Electrochemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Manufacturing & Machinery (AREA)
  • Inorganic Chemistry (AREA)
  • Materials Engineering (AREA)
  • Composite Materials (AREA)
  • Physics & Mathematics (AREA)
  • Condensed Matter Physics & Semiconductors (AREA)
  • General Physics & Mathematics (AREA)
  • Dispersion Chemistry (AREA)
  • Secondary Cells (AREA)
  • Battery Electrode And Active Subsutance (AREA)
PCT/US2020/021527 2019-03-06 2020-03-06 Rechargeable li-ion battery with halogen intercalated graphite electrode Ceased WO2020181244A1 (en)

Priority Applications (7)

Application Number Priority Date Filing Date Title
CN202080018985.4A CN113544878B (zh) 2019-03-06 2020-03-06 卤素嵌入石墨电极的可充电锂离子电池
EP20766129.9A EP3935680A4 (en) 2019-03-06 2020-03-06 Rechargeable li-ion battery with halogen intercalated graphite electrode
KR1020217031016A KR102813666B1 (ko) 2019-03-06 2020-03-06 할로겐 인터칼레이션된 그래파이트 전극을 갖는 충전식 리튬 이온 배터리
US17/436,609 US12142722B2 (en) 2019-03-06 2020-03-06 Rechargeable Li-ion battery with halogen intercalated graphite electrode
CN202510730513.6A CN120581728A (zh) 2019-03-06 2020-03-06 卤素嵌入石墨电极的可充电锂离子电池
KR1020257016994A KR20250084228A (ko) 2019-03-06 2020-03-06 할로겐 인터칼레이션된 그래파이트 전극을 갖는 충전식 리튬 이온 배터리
JP2021552631A JP7599221B2 (ja) 2019-03-06 2020-03-06 ハロゲンインターカレーション黒鉛電極を備えた充電式Liイオン電池

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US201962814618P 2019-03-06 2019-03-06
US62/814,618 2019-03-06

Publications (1)

Publication Number Publication Date
WO2020181244A1 true WO2020181244A1 (en) 2020-09-10

Family

ID=72338454

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2020/021527 Ceased WO2020181244A1 (en) 2019-03-06 2020-03-06 Rechargeable li-ion battery with halogen intercalated graphite electrode

Country Status (6)

Country Link
US (1) US12142722B2 (enExample)
EP (1) EP3935680A4 (enExample)
JP (1) JP7599221B2 (enExample)
KR (2) KR102813666B1 (enExample)
CN (2) CN120581728A (enExample)
WO (1) WO2020181244A1 (enExample)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2022057278A1 (zh) * 2020-09-21 2022-03-24 江苏正力新能电池技术有限公司 一种快充石墨及电池
JPWO2022219847A1 (enExample) * 2021-04-15 2022-10-20

Families Citing this family (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR20240128866A (ko) * 2021-12-20 2024-08-27 유니버시티 오브 매릴랜드, 칼리지 파크 증가된 전기화학적 안정성 창을 갖는 Li-이온 배터리
KR102819934B1 (ko) * 2022-08-16 2025-06-13 한양대학교 산학협력단 염중수 전해액 중 양전위 전극의 물이 배제된 계면층을 인식하는 전기화학 분석법
US12540917B2 (en) 2022-08-16 2026-02-03 Iucf-Hyu (Industry-University Cooperation Foundation Hanyang University) Electrochemical analysis method of recognizing interfacial layer with depleted water on positively electrified electrode in water-in-salt
CN116135788B (zh) * 2023-03-13 2023-11-14 浙江师范大学 一种卤素插层的五氧化二钒纳米花的制备方法、产品及应用
JP2026517504A (ja) * 2023-05-23 2026-06-01 ユニバーシティ オブ メリーランド, カレッジ パーク 再充電可能な複合電極及びその方法
CN119764759B (zh) * 2024-12-12 2026-02-03 深圳大学 一种负载嵌锂态石墨的聚合物膜及其制备方法和应用、含硅负极的锂离子电池

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20150037680A1 (en) * 2013-07-31 2015-02-05 Samsung Electronics Co., Ltd. Composite cathode active material, lithium battery including the same, and preparation method thereof
US20180219214A1 (en) * 2017-01-30 2018-08-02 Nanotek Instruments.com Exfoliated Graphite Worm-Protected Metal Fluoride and Metal Chloride Cathode Active Materials for Lithium Batteries

Family Cites Families (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4009323A (en) 1975-05-12 1977-02-22 The United States Of America As Represented By The Secretary Of The Navy Storage battery comprising positive electrode of a graphite and lithium fluoride compound
WO2006128174A2 (en) 2005-05-26 2006-11-30 California Institute Of Technology High voltage and high specific capacity dual intercalating electrode li-ion batteries
WO2008047898A1 (fr) * 2006-10-20 2008-04-24 Ishihara Sangyo Kaisha, Ltd. dispositif de stockage
TWI469435B (zh) 2013-04-17 2015-01-11 Taiwan Carbon Nanotube Technology Corp Seawater battery
US9509017B2 (en) 2014-07-22 2016-11-29 John E. Stauffer Lithium storage battery
KR20160015708A (ko) * 2014-07-31 2016-02-15 주식회사 엘지화학 희생 염을 포함하는 리튬 이차전지
CN108431997A (zh) * 2015-07-13 2018-08-21 新罗纳米技术有限公司 用于金属和金属离子电池的稳定的氟化锂基阴极
US10916766B2 (en) * 2017-04-10 2021-02-09 Global Graphene Group, Inc. Alkali metal-sulfur secondary battery containing a polymer-encapsulated sulfur cathode and manufacturing method
JP6562043B2 (ja) 2017-07-26 2019-08-21 トヨタ自動車株式会社 水系デュアルイオン二次電池
CN109309244B (zh) 2017-07-27 2021-08-24 南京工业大学 一种混合水性可充电电池
US11876178B2 (en) * 2017-08-25 2024-01-16 University Of Maryland, College Park High voltage aqueous electrolyte system for lithium metal or graphite anode

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20150037680A1 (en) * 2013-07-31 2015-02-05 Samsung Electronics Co., Ltd. Composite cathode active material, lithium battery including the same, and preparation method thereof
US20180219214A1 (en) * 2017-01-30 2018-08-02 Nanotek Instruments.com Exfoliated Graphite Worm-Protected Metal Fluoride and Metal Chloride Cathode Active Materials for Lithium Batteries

Non-Patent Citations (3)

* Cited by examiner, † Cited by third party
Title
CHONGYIN YANG; CHEN JI; QING TINGTING; FAN XIULIN; SUN WEI; VON CRESCE ARTHUR; DING MICHAEL S; BORODIN OLEG; VATAMANU JENEL; SCHRO: "4.0 V aqueous Li-ion batteries", JOULE, vol. 1, no. 1, 6 September 2017 (2017-09-06), pages 122 - 132, XP055578152, ISSN: 2542-4351, DOI: 10.1016/j.joule.2017.08.009 *
MENG-CHANG LIN, MING GONG, BINGAN LU, YINGPENG WU, DI-YAN WANG, MINGYUN GUAN, MICHAEL ANGELL, CHANGXIN CHEN, JIANG YANG, BING-JOE : "An ultrafast rechargeable aluminium-ion battery", NATURE, vol. 520, 6 April 2015 (2015-04-06), pages 324 - 328, XP055184163, ISSN: 0028-0836, DOI: 10.1038/nature14340 *
See also references of EP3935680A4 *

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2022057278A1 (zh) * 2020-09-21 2022-03-24 江苏正力新能电池技术有限公司 一种快充石墨及电池
JPWO2022219847A1 (enExample) * 2021-04-15 2022-10-20
JP7918990B2 (ja) 2021-04-15 2026-09-11 パナソニックIpマネジメント株式会社 固体電解質材料およびそれを用いた電池

Also Published As

Publication number Publication date
CN113544878A (zh) 2021-10-22
CN113544878B (zh) 2025-06-20
US12142722B2 (en) 2024-11-12
CN120581728A (zh) 2025-09-02
JP2022523977A (ja) 2022-04-27
KR20250084228A (ko) 2025-06-10
KR102813666B1 (ko) 2025-05-28
US20220131180A1 (en) 2022-04-28
EP3935680A4 (en) 2024-09-18
KR20210135262A (ko) 2021-11-12
EP3935680A1 (en) 2022-01-12
JP7599221B2 (ja) 2024-12-13

Similar Documents

Publication Publication Date Title
Yang et al. Aqueous Li-ion battery enabled by halogen conversion–intercalation chemistry in graphite
US12142722B2 (en) Rechargeable Li-ion battery with halogen intercalated graphite electrode
Liu et al. Rechargeable anion-shuttle batteries for low-cost energy storage
Zhao et al. Stabilizing metal battery anodes through the design of solid electrolyte interphases
Shang et al. An “Ether‐in‐Water” electrolyte boosts stable interfacial chemistry for aqueous lithium‐ion batteries
Cheng et al. Electrolyte salts for sodium-ion batteries: NaPF6 or NaClO4?
Wang et al. Challenges and progress in rechargeable magnesium‐ion batteries: materials, interfaces, and devices
US12057556B2 (en) Aqueous and hybrid electrolytes with wide electrochemical stability windows
KR102470117B1 (ko) 충전식 배터리 셀
Li et al. Anthraquinone-based silicate covalent organic frameworks as solid electrolyte interphase for high-performance lithium–metal batteries
Muldoon et al. Quest for nonaqueous multivalent secondary batteries: magnesium and beyond
Moon et al. Mechanism of Li ion desolvation at the interface of graphite electrode and glyme–Li salt solvate ionic liquids
CN101467287B (zh) 氟离子电化学电池
Adams et al. Mechanistic elucidation of thermal runaway in potassium-ion batteries
Zhang et al. Li+ (ionophore) nanoclusters engineered aqueous/non-aqueous biphasic electrolyte solutions for high-potential lithium-based batteries
Kaland et al. Are MXenes suitable as cathode materials for rechargeable Mg batteries?
Jayakumar et al. Allylimidazolium-based poly (ionic liquid) anodic binder for lithium-ion batteries with enhanced cyclability
KR102628721B1 (ko) 나노입자 재료 및 불화물 이온 배터리의 제조 방법
Kim et al. Achieving high-performance Li–S batteries via polysulfide adjoining interface engineering
EP3614481A1 (en) Polymer electrolyte composition, and polymer secondary battery
Su et al. Potential complexes of NaCF3SO3-tetraethylene dimethyl glycol ether (tetraglyme)-based electrolytes for sodium rechargeable battery application
Fan et al. Surface-dipole-directed formation of stable solid electrolyte interphase
Qiu et al. Fluorine/sulfur-comodulated covalent organic frameworks cathode for high-performance lithium ion batteries
JP2013065534A (ja) 層状化合物及びそれを用いた蓄電池
US20190355992A1 (en) Cathode stabilization method using electrochemical oxidative additives in aqueous alkali-ion batteries

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 20766129

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2021552631

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 20217031016

Country of ref document: KR

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 2020766129

Country of ref document: EP

Effective date: 20211006

WWG Wipo information: grant in national office

Ref document number: 202127040301

Country of ref document: IN

WWP Wipo information: published in national office

Ref document number: 1020257016994

Country of ref document: KR

WWG Wipo information: grant in national office

Ref document number: 202080018985.4