WO2009151825A2 - Transition metal initiators supported by ketone diimine ligands for the homopolymerization of olefins and the copolymerization of olefins with polar comonomers - Google Patents

Transition metal initiators supported by ketone diimine ligands for the homopolymerization of olefins and the copolymerization of olefins with polar comonomers Download PDF

Info

Publication number
WO2009151825A2
WO2009151825A2 PCT/US2009/042877 US2009042877W WO2009151825A2 WO 2009151825 A2 WO2009151825 A2 WO 2009151825A2 US 2009042877 W US2009042877 W US 2009042877W WO 2009151825 A2 WO2009151825 A2 WO 2009151825A2
Authority
WO
WIPO (PCT)
Prior art keywords
alkyl
polymerization
complex
olefins
aryl
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2009/042877
Other languages
English (en)
French (fr)
Other versions
WO2009151825A3 (en
Inventor
Jason D. Azoulay
Yanika Schneider
Guillermo C. Bazan
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of California Berkeley
University of California, San Diego
Original Assignee
University of California Berkeley
University of California, San Diego
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of California Berkeley, University of California, San Diego filed Critical University of California Berkeley
Priority to JP2011510554A priority Critical patent/JP5651107B2/ja
Priority to CN2009801182998A priority patent/CN102037025B/zh
Priority to EP09763116.2A priority patent/EP2288626A4/en
Publication of WO2009151825A2 publication Critical patent/WO2009151825A2/en
Publication of WO2009151825A3 publication Critical patent/WO2009151825A3/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C07—ORGANIC CHEMISTRY
    • C07F—ACYCLIC, CARBOCYCLIC OR HETEROCYCLIC COMPOUNDS CONTAINING ELEMENTS OTHER THAN CARBON, HYDROGEN, HALOGEN, OXYGEN, NITROGEN, SULFUR, SELENIUM OR TELLURIUM
    • C07F15/00—Compounds containing elements of Groups 8, 9, 10 or 18 of the Periodic Table
    • C07F15/04—Nickel compounds
    • C07F15/045—Nickel compounds without a metal-carbon linkage
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F10/00—Homopolymers and copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F110/00—Homopolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F110/02—Ethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F110/00—Homopolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F110/04—Monomers containing three or four carbon atoms
    • C08F110/06—Propene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F210/00—Copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F210/02—Ethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F210/00—Copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F210/16—Copolymers of ethene with alpha-alkenes, e.g. EP rubbers

Definitions

  • the present invention relates generally to polymers, and more particularly to organometallic initiators capable of polymerizing and copolymerizing olefins.
  • Examples of how the metal center can tailor properties by controlling monomer insertion include the stereo specific polymerization of propene (8, 9, 10, 11, 12, 13, 14) and the copolymerization of ethylene and 1-alkenes (15, 16, 17, 18).
  • the design of late transition metal initiators has received renewed interest because of their lower oxophilicity and resistance toward deactivation by polar functionalities, relative to their early transition metal counterparts (19, 20, 21, 22, 23). This reduced sensitivity of late metals to polar impurities allows for polymerizations to be carried out under less stringent conditions and allows for the copolymerization with polar comonomers (24, 25, 26, 27, 28).
  • Nickel and palladium based catalysts have been shown to participate in chain walking reactions (29, 30, 31), tolerate polar functionalities (24, 25, 26, 27, 28) and have even been used in water (32, 33, 34). These catalytic properties are of significant interest for developing materials with unique properties and for the development of new commercial processes.
  • ethylene sequences (18, 54) can be generated from the chain straightening of higher ⁇ -olefins (3, 30, 51, 52, 53).
  • novel materials such as elastomeric multi-block poly( ⁇ -olefins) (54), ethylene-propylene type copolymers (18), regioblock copolymers (18, 55, 56), and end-functionalized amorphous PE (24).
  • a novel ligand metal combination or initiator.
  • the initiator Upon activation with various co-catalysts, the initiator polymerizes ethylene and propylene, and/or other olefin monomers, to high molecular weight polymers.
  • the copolymerization of olefins with functionalized comonomers can be carried out. In some embodiments, polymerization can be carried out in a living manner.
  • the general initiator structure comprises a late transition metal with a neutral chelating ligand that contains a Lewis basic functionality.
  • the general initiator structure comprises the following formula (I):
  • R, R', R" and R'" are each independently an achirai or chiral alkyl or aryl group with or without one or more functional groups;
  • M is Fe, Co, Ni, Pd or Pt
  • X is an alkyl, hydride or halide group
  • R and R' are each alkyl, and R" and R 1 " are each aryl; embodiments in which L is O; embodiments in which L is O, R and R' are each alkyl, and R" and R"' are each aryl; embodiments in which R and R' are each methyl, and R" and R'" are each aryl, including embodiments where L is O; embodiments in which R and R' are each alkyl, and R" and R'” are each 2,6 disubstituted aryl, including embodiments where L is O; and embodiments in which the initiator is 2,4-bis(2,6- diisopropylphenylimino)pentan-3-one nickel dibromide, or 2,4-bis(2-isopropyl-6- methylphenylimino)pentan-3-one nickel dibromide.
  • a process of producing an organometallic initiator complex comprising mixing a metal compound with a ligand of the following formula (II)
  • R and R' are each alkyl, and R" and R"' are each aryl; embodiments in which L is O; embodiments in which L is O, R and R' are each alkyl, and R" and R"' are each aryl; embodiments in which R and R' are each methyl, and R" and R'" are each aryl, including embodiments where L is O; embodiments in which R and R' are each alkyl, and R" and R'” are each 2,6 disubstituted aryl, including embodiments where L is O; and embodiments in which R" and R'" are each 2,6- diisopropylphenyl or 2-isopropyl-6-methylphenyl.
  • the process producing an organometallic complex utilizes a metal halide complex as the metal compound, which in certain embodiments is a (1,2- dimethoxyethane)NiBr 2 complex.
  • a polymerization process comprises mixing one, or more than one, olefin with an organometallic complex so as to produce a polymer that comprises the one, or more than one, olefin.
  • the organometallic complex has the structure of formula (I), or any embodiments of formula (I).
  • R and R' are each alkyl, and R" and R'" are each aryl; embodiments in which L is O; embodiments in which L is O, R and R' are each alkyl, and R" and R'" are each aryl; embodiments in which R and R' are each methyl, and R" and R 1 " are each aryl, including embodiments where L is O; embodiments in which R and R 1 are each alkyl, and R" and R'” are each 2,6 disubstituted aryl, including embodiments where L is O; and embodiments in which the organometallic complex is 2,4- bis(2,6-diisopropylphenylimino)pentan-3-one nickel dibromide, or 2,4-bis(2-isopropyl-6- methylphenylimino)pentan-3-one nickel dibromide.
  • Examples of X include, but are not limited to: a halogen such as Cl, Br, or F; -CN; -C 6 H 5 N; -CONR 3 R 4 ; -OR 3 ; -COOR 3 ; -OCOR 3 ; -COR 3 ; -C 6 H 5 OR 3 ; and/or -C 6 H 5 NR 3 R 4 ; wherein R 3 and R 4 are each independently hydrogen or an alkyl group, which can be a Ci -I2 alkyl group.
  • a halogen such as Cl, Br, or F
  • the polymerization process utilizes a single olefin, such as any one of the olefins described herein, resulting in homopolymerization.
  • the polymerization process utilizes two or more than two different olefins, which can include at least one or any combination of the olefins described herein, resulting in copolymerization.
  • the polymerization process can be carried out under living polymerization conditions such that a polymer is produced by a living polymerization process.
  • the use of two, three or more than three different monomers, which can include at least one or any combination of the olefins described herein, can produce a block copolymer.
  • a co-catalyst is used.
  • the co-catalyst can be added to any embodiment of the polymerization process, and can be an alkylaluminum, aluminoxane, or borate compound.
  • the polymerization products produced by the polymerization process include semicrystalline polymers.
  • Figure 1 is an ORTEP drawing of initiator 1 at the 50% probability level
  • Figure 2 is a graph of the IR spectras of copolymers showing incorporation of methyl acrylate into polyethylene
  • Figure 3 is a graph showing optimization of cocatalyst with the initiator in polymerization experiments
  • Figure 4 is a table illustrating the larger scale polymerization of ethylene with initiator 1;
  • Figure 5 is a table illustrating the larger scale copolymerization of ethylene and acrylates with initiator 1 ;
  • Figure 6 is a table illustrating the larger scale copolymerization of ethylene and 1- hexene;
  • Figure 7 is a differential scanning calorimetry trace of a semicrystalline polypropylene;
  • Figure 8A is a scheme showing the synthesis of polyethylene (PE), polypropylene (PP) and poly(l-hexene) with symmetric GPC traces and polydispersities less than 1.1 using initiator 1/MAO at low temperatures
  • Figure 8B is a graph showing GPC traces for various polymers
  • Figure 9 shows a plot of M n versus time for various polymers.
  • Novel organometallic initiator complexes are provided that are capable of polymerizing olefins or copolymerizing olefins with functional ized comonomers to yield high molecular weight polymers (>5,000).
  • the initiator is 2,4-bis(2,6-diisopropylphenylimino)pentan-3-one nickel dibromide or 2,4-bis(2-isopropyl-6-methylphenylimino)pentan-3-one nickel dibromide.
  • alkyl refers to a branched or unbranched saturated hydrocarbyl group such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, octyl, decyl, and the like, as well as cycloalkyl groups such as cyclopentyl, cyclohexyl and the like.
  • an alkyl group can be Ci -30 or Ci -20 .
  • aryl refers to an aromatic hydrocarbyl group containing a single aromatic ring or multiple aromatic rings that are fused together, linked covalently, or linked to a common group such as a methylene or ethylene moiety.
  • aryl groups contain one aromatic ring or two fused or linked aromatic rings, e.g., phenyl, naphthyl, biphenyl, diphenylether, diphenylamine, benzophenone, and the like.
  • an aryl group including any substituents can have from 4 to 50 carbon atoms, 4 to 40 carbon atoms, 4 to 30 carbon atoms, 4 to 20 carbon atoms, or 4 to 10 carbon atoms, or more particularly, can have from 6 to 50 carbon atoms, 6 to 40 carbon atoms, 6 to 30 carbon atoms, 6 to 20 carbon atoms or 6 to 10 carbon atoms.
  • alkoxy refers to an alkyl group bound through a single, terminal ether linkage; that is, an alkoxy group may be represented as — O-alkyl, where alkyl is as defined above.
  • an alkyl group or an aryl group can be substituted with a functional group.
  • substituted in connection with a hydrocarbyl group refers to a hydrocarbyl group in which at least one hydrogen atom bound to a carbon atom is replaced with one or more substituents.
  • a disubstituted aryl group such as a diisopropylphenyl group, has two substituents replacing two hydrogen atoms of the parent aryl group.
  • a substituent can be a "functionality" or “functional group” such as, but not limited to, halo, ester, keto (oxo), amino, imino, hydroxyl, carboxyl, phosphite, phosphonite, phosphine, phosphinite, thioether, amide, nitrile, and ether.
  • methyl acrylate can be considered a hydrocarbyl substituted with a carboxyl functional group.
  • an alkyl or aryl group can have one, two, three, four, or more than four, substituents.
  • R, R', R" and R' can each independently be an achiral or chiral hydrocarbyl group.
  • chiral refers to molecules which have the property of non-superimposability on their mirror image partner
  • achiral refers to molecules which are superimposable on their mirror image partner.
  • Initiators can be prepared by combining a ligand with an appropriate metal.
  • the initiators are prepared via a reaction sequence, as shown in Example 1 (below).
  • a general formula (II) of such a ligand is as follows:
  • R 1 can be hydrogen, alkyl, or a substituted alkyl bearing one or more functional groups (such as, -OH, -NH 2 , -CN, -COOR, -OCOR, -C(O)R, or -C(O)NRR', where R and R' are each independently hydrogen or an alkyl group).
  • functional groups such as, -OH, -NH 2 , -CN, -COOR, -OCOR, -C(O)R, or -C(O)NRR', where R and R' are each independently hydrogen or an alkyl group).
  • Examples of X include, but are not limited to: a halogen such as Cl, Br, or F; -CN; -C 6 H 5 N; -CONR 3 R 4 ; -OR 3 ; -COOR 3 ; -OCOR 3 ; -C 6 H 5 OR 3 ; -COR 3 and/or -C 6 H 5 NR 3 R 4 ; wherein R 3 and R 4 are each independently hydrogen or an alkyl group, which can be a CM 2 alkyl group.
  • Polymers generated in connection with these initiators can exhibit a unique microstructure.
  • Polymerizations can occur at temperatures from at or about -100 0 C to at or about 250 0 C. The preferred range is at or about 60 0 C to at or about 200 0 C.
  • these initiators can be used for copolymerization of ethylene with functional ized comonomers (as in Example 4, below) or other 1-alkenes.
  • Co-catalysts can be used with the above initiators for polymerization/copolymerization reactions.
  • Such co-catalysts include, but are not limited to, any alkylaluminum, alkylaluminoxane, and borate co-catalyst known in the art.
  • Such co- catalysts include, but are not limited to, methylaluminoxane (MAO), modified methylaluminoxane type-3A, or trimethylaluminum (TMA).
  • polymerization can occur under conditions that result in a living polymerization process.
  • a single monomer can be polymerized in a living manner, or more than one monomer can undergo living polymerization.
  • living polymerization can occur so that the growth of M n of the polymer as a function of time is linear.
  • molecular weight distributions that are symmetric and polymers with PDI values of less than or equal to 1.3 can be obtained.
  • block copolymers including diblock, triblock and other multiblock copolymers
  • a first monomer can be polymerized to produce a polymer product, and then a second monomer can be added to the polymer product to produce a block copolymer.
  • tapered, regioblock and/or end functionalized polymers can be prepared.
  • Polymerization under living conditions can also yield semicrystalline polymers such as semicrystalline polyethylene or polypropylene.
  • semicrystalline refers to polymers that have both a crystalline portion and an amorphous portion. Polymerization under living conditions can also yield amorphous polymers.
  • Initiator 1 is synthesized from the ligand, 2,4-bis(2,6-diisopropylphenylimino)pentan- 3-one.
  • This ligand can be made according the following scheme and procedure.
  • [Cu"( I)AcO] (5 g) was treated in methanol (1000 mL) at 50 0 C in a 3 neck round bottom flask capped with two septa and a reflux condensor attached to an oil bubbler. Oxygen was vigorously bubbled through the solution for 72 hours or until a complete color change from brown to purple was noted. At this point oxygen was bubbled through for another 12 hours and the volume was reduced to 100 mL by bubbling oxygen through at 50 0 C. The methanol solution was cooled by allowing to stand at room temperature, overnight, under an atmosphere of oxygen. Purple crystals were collected by filtration.
  • initiator 1 was carried out under an inert atmosphere according to Scheme 1. All reagents were dried, by various methods, prior to use.
  • Homopolymerizations of ethylene were conducted in the following manner using initiator 1.
  • a 300 mL steel autoclave reactor, equipped with an addition funnel was loaded, inside a glovebox with initiator 1 in 90 mL of toluene.
  • Methylaluminoxane (Aldrich, 10 wt. % in toluene) (MAO) was added to the addition funnel followed by toluene so that the final volume was 10 mL.
  • the reactor was sealed inside the glovebox and attached to an ethylene line.
  • the reactor was pre-pressurized with ethylene.
  • the MAO solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction.
  • Polymer melting points were measured on a TA instruments differential scanning calorimeter, (model DSC 2920) at a rate of 10 °C/min for three cycles using a temperature range of 0 - 180 0 C.
  • the optimal amount of co-catalyst (MAO) was determined as shown in Figure 3.
  • Table 1 shows selected polymerization data.
  • Homopolymerizations of propene were conducted in the following manner using initiator 1.
  • a 300 mL steel autoclave reactor, equipped with an addition funnel was loaded, inside a glovebox with initiator 1 in 90 mL of toluene.
  • MAO Aldrich, i0 wt. % in toluene
  • the reactor was sealed inside the glovebox and attached to a propene line.
  • the reactor was pre-pressurized with propene.
  • the MAO solution was then injected under a specified pressure of propene, which was fed continuously at that pressure over the course of the reaction.
  • the polypropylene produced is mainly amorphous with T g s ranging from - 35 0 C to - 20 0 C depending on the reaction temperature. Entry 1, 2 and 4 exhibit the following tacticity as illustrated in Table 3, below.
  • EXAMPLE 4 Copolymerization of Ethylene and Methyl Acrylate
  • Copolymerizations of ethylene and methyl acrylate were conducted in the following manner using initiator 1.
  • a 300 mL steel autoclave reactor, equipped with an addition funnel was loaded, inside a glovebox with initiator 1 in 90 mL of toluene.
  • MAO Aldrich, 10 wt. % in toluene
  • the reactor was sealed inside the glovebox and attached to an ethylene line.
  • the reactor was pre-pressurized with ethylene.
  • the MAO - methyl acrylate solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction. Ethylene was vented after a specified amount of time and acidified methanol (10 % HCl) was added to quench the polymerization. The precipitated polymer was collected by centrifugation, washed copiously with methanol, followed by THF. and dried under high vacuum overnight. Polymerization activities were calculated from the mass of the product obtained. Polymers were characterized by GPC analysis, relative to polystyrene standards, at 135 0 C in o-dichlorobenzene (in a Polymer Laboratories, high-temperature chromatograph, Pl-GPC 200). 1 H NMR spectra of the polymers was obtained in 1,1, 2,2-tetrachloroethane-cfe at 1 15 0 C.
  • Homopolymerizations of ethylene were conducted in the following manner using initiator 1.
  • a 2000 mL steel autoclave reactor, equipped with an addition straw was heated in an oven at 150 0 C overnight.
  • the reactor was assembled, while hot and purged with nitrogen and pumped down a total of three times.
  • the reactor was then sealed under nitrogen.
  • a specified amount of solvent and co-catalyst were added using standard Schlenk and air-free techniques.
  • a stock solution of the initiator was prepared and added to the addition straw under a stream of nitrogen.
  • the reactor was sealed and attached to an ethylene line.
  • the reactor was pre-pressurized with ethylene.
  • the initiator solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction.
  • Figure 4 shows selected polymerization data obtained from the homopolymerization of ethylene, and illustrates the following.
  • the ethylene consumption is consistent over the course of 30 minutes.
  • the activity is significantly higher when MMA0-3A is used as a co- catalyst versus MAO.
  • Copolymerizations of ethylene and methyl or t-butyl acrylate were conducted in the following manner using initiator 1.
  • a 2000 mL steel autoclave reactor, equipped with an addition straw was heated in an oven at 150 °C overnight.
  • the reactor was assembled, while hot and purged with nitrogen and pumped down a total of three times.
  • the reactor was then sealed under nitrogen.
  • a specified amount of solvent, co-catalyst and acrylate were added using standard Schlenk and air-free techniques.
  • Acrylate was added to give 0.082 M solution in reaction 14 and 15.
  • a stock solution of the initiator was prepared and added to the addition straw.
  • the reactor was sealed and attached to an ethylene line.
  • the reactor was pre- pressurized with ethylene.
  • the initiator solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction. 10 mL ethanol was added to quench the polymerization. The precipitated polymer was collected by filtration, washed copiously with acidified methanol (10 % HCI); then washed with methanol followed by acetone and dried in a vacuum oven overnight. Polymerization activities were calculated from the mass of the product obtained. Polymers were characterized by GPC analysis, relative to polystyrene standards, at 135 0 C in o- dichlorobenzene (in a Polymer Laboratories, high-temperature chromatograph, Pl-GPC 200). 1 H and 13 C NMR spectra of the polymers was obtained in l,l,2,2-tetrachloroethane-c/ 2 at 115 0 C.
  • Figure 5 shows the results of copolymerizations using ethylene and acrylates.
  • the figure illustrates that the copolymerization of ethylene and methyl acrylate proceeds with good activity in the presence of MMAO at 50 0 C and 3.0 MPag.
  • the incorporation of methyl acrylate was 0.14 mol % in reaction 14.
  • this illustrates that the choice of co-catalyst and reaction conditions are important for activity, incorporation and polymer microstructure. Under the same conditions, the copolymerization of ethylene and tert-butyl acrylate showed lower activity and less incorporation.
  • Copolymerizations of ethylene and 1-hexene were conducted in the following manner using initiator 1.
  • a 2000 mL steel autoclave reactor, equipped with an addition straw was heated in an oven at 150 0 C overnight.
  • the reactor was assembled, while hot and purged with nitrogen and pumped down a total of three times.
  • the reactor was then sealed under nitrogen.
  • a specified amount of solvent, co-catalyst and 50 mL 1-hexene were added using standard Schlenk and air-free techniques.
  • a stock solution of the initiator was prepared and added to the addition straw.
  • the reactor was sealed and attached to an ethylene line.
  • the reactor was pre-pressurized with ethylene.
  • the initiator solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction. 10 mL ethanol was added to quench the polymerization. The precipitated polymer was collected by filtration, washed copiously with acidified methanol (10 % HCl); then washed with methanol followed by acetone and dried in a vacuum oven overnight. Polymerization activities were calculated from the mass of the product obtained. Polymers were characterized by GPC analysis, relative to polystyrene standards, at 135 0 C in o- dichlorobenzene (in a Polymer Laboratories, high-temperature chromatograph, Pl-GPC 200). 1 H and 13 C NMR spectra of the polymers was obtained in 1,1, 2,2-tetrachloroethane-c/ 2 at 115 0 C.
  • initiator 2 was carried out according to Scheme 2 under an inert atmosphere. All reagents were dried, by various methods, prior to use.
  • Homopolymerizations of ethylene were conducted in the following manner using initiator 2.
  • a 300 mL steel autoclave reactor, equipped with an addition funnel was loaded, inside a glovebox with initiator 2 in 90 mL of toluene.
  • MAO Aldrich, 10 wt. % in toluene
  • the reactor was sealed inside the glovebox and attached to an ethylene line.
  • the reactor was pre-pressurized with ethylene.
  • the MAO solution was then injected under a specified pressure of ethylene, which was fed continuously at that pressure over the course of the reaction.
  • Polymer melting points were measured on a TA instruments differential scanning calorimeter, (model DSC 2920) at a rate of 10 °C/min for three cycles using a temperature range of 0 - 180 0 C. Table 5 below shows selected polymerization data.
  • FIG. 7 shows a differential scanning calorimetry generated graph for entry 2 in Table 6 above.
  • the melting temperature (T m ) and corresponding crystallization temperature (T c ) indicate the transition from a purely amorphous polymer to a polymer with some crystallinity based on the symmetry of the ligand and the reaction conditions. This illustrates that the microstructure can be controlled based on the choice of ligand and the corresponding reaction conditions.
  • Examples 12-15 relate to living polymerization reactions.
  • Example 12 describes the results of polymerization reactions, while Examples 13-15 provide supporting information for the results described in Example 12.
  • Reaction time minutes
  • temperature 0 C
  • turnover frequency TOF
  • Figure 8B shows GPC traces for PE, PP and PH under the conditions in Table 7, entries 8, 9 and 10, respectively.
  • Figure 9 shows a plot of M n versus time under the same conditions as in entry 7 (M n ( ⁇ ) and PDI (x) versus time using initiator 1/MAO at -10 0 C for PE, PP and PH determined by GPC).
  • the linear growth of M n as a function of time and PDI values ⁇ 1.10, together with the results in Table 7, are consistent with the formation of semicrystalline PE under living conditions.
  • the method described herein provides conditions that allow for the living polymerization of ethylene and ⁇ -olefins by using initiator 1/MAO. This is apparently the first late metal system that can polymerize ethylene in a living manner to afford semicrystalline PE, in contrast to quasi-living polymerization such as that in Diamanti et al. (25). This excellent control is remarkable given the fact that the PE precipitates over the course of the reaction. Additionally, it is interesting to note that the PP produced contains isotactic sequences.
  • Reagents unless otherwise specified, were purchased from Aldrich and used without further purification. Polymerization activities were calculated from the mass of the product obtained. Polymers were characterized by GPC analysis, relative to polystyrene standards, at 135 °C in o-dichlorobenzene (in a Varian Polymer Laboratories, high-temperature chromatograph, PL GPC 220). Polymer melting points (T m ) and glass transition temperatures (7 ⁇ ) were measured on a TA Instruments differential scanning calorimeter (model Q-20) at a rate of 10 °C/min for three cycles using a temperature range of -70 to 180 0 C.
  • the addition funnel was pre-pressurized with ethylene at 50 psi above the desired reaction pressure with ethylene.
  • the reactor was pre-pressurized to ⁇ PC2H 4 ) with ethylene and cooled to the appropriate reaction temperature (T mn ).
  • the polymerization was initiated via injection of the solution of initiator 1 and ethylene was continually fed into the reactor over the course of the reaction.
  • the reaction temperature (T nn ) was controlled using a dry-ice/acetone bath and found to be ⁇ 2 0 C as monitored by an internal thermocouple. Ethylene was vented after a specified amount of time, and methanol was added to quench the polymerization (entries 1- 6).
  • the polymer was precipitated with methanol and was collected by filtration and washed with acidified methanol (10% HCl), methanol and acetone sequentially and dried under high vacuum to constant weight.
  • the activity of the polymerization was calculated from the mass of the product obtained.
  • reactions utilizing triethylsilane (Et 3 SiH) as the quenching agent (Table 7, entries 7 & 8 and Table 8)
  • 1 mL Et 3 SiH in 2 mL of toluene was added to the addition funnel following introduction of the initiator stock solution.
  • the addition funnel was pre-pressurized with ethylene at 50 psi above the desired reaction pressure (Pc 2H d and the solution injected into the rapidly stirring reaction mixture at the appropriate time point.
  • Table 8 Living Polymerization of Ethylene.
  • the reaction temperature (T nn ) was controlled by means of a dry-ice/acetone bath and found to be ⁇ 2 0 C as monitored by an internal thermocouple.
  • M n number average molecular weight
  • PDI polydispersity
  • the reaction temperature [T nn ) was controlled by means of a dry-ice/acetone bath and found to be ⁇ 2 °C as monitored by an internal thermocouple.
  • M n number average molecular weight
  • PDI polydispersity

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Transition And Organic Metals Composition Catalysts For Addition Polymerization (AREA)
  • Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
PCT/US2009/042877 2008-05-19 2009-05-05 Transition metal initiators supported by ketone diimine ligands for the homopolymerization of olefins and the copolymerization of olefins with polar comonomers Ceased WO2009151825A2 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2011510554A JP5651107B2 (ja) 2008-05-19 2009-05-05 オレフィンの単一重合のためのケトンジイミンリガンドに担持された遷移金属開始剤及び極性コモノマーを用いたオレフィンの共重合
CN2009801182998A CN102037025B (zh) 2008-05-19 2009-05-05 用于烯烃均聚以及烯烃与极性共聚单体共聚的、负载于酮二亚胺配体的过渡金属引发剂
EP09763116.2A EP2288626A4 (en) 2008-05-19 2009-05-05 TRANSITION METAL INITIATORS SUPPORTED BY KETONDIIMINLIGANES FOR THE HOMOPOLYMERIZATION OF OLEFINES AND THE COPOLYMERIZATION OF OLEFINS WITH POLAR COMONOMERS

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US12817408P 2008-05-19 2008-05-19
US61/128,174 2008-05-19

Publications (2)

Publication Number Publication Date
WO2009151825A2 true WO2009151825A2 (en) 2009-12-17
WO2009151825A3 WO2009151825A3 (en) 2010-02-04

Family

ID=41380615

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2009/042877 Ceased WO2009151825A2 (en) 2008-05-19 2009-05-05 Transition metal initiators supported by ketone diimine ligands for the homopolymerization of olefins and the copolymerization of olefins with polar comonomers

Country Status (5)

Country Link
US (1) US8242297B2 (cg-RX-API-DMAC7.html)
EP (1) EP2288626A4 (cg-RX-API-DMAC7.html)
JP (1) JP5651107B2 (cg-RX-API-DMAC7.html)
CN (1) CN102037025B (cg-RX-API-DMAC7.html)
WO (1) WO2009151825A2 (cg-RX-API-DMAC7.html)

Families Citing this family (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN104177528B (zh) * 2014-07-23 2016-08-24 浙江大学 一种乙烯/长链α-烯烃共聚物及其制备方法
CN119350399A (zh) * 2023-07-24 2025-01-24 中国石油天然气股份有限公司 一种两性离子型烯丙基镍配合物及其制备方法与应用

Family Cites Families (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5880241A (en) * 1995-01-24 1999-03-09 E. I. Du Pont De Nemours And Company Olefin polymers
JP3847783B2 (ja) * 1995-01-24 2006-11-22 イー・アイ・デュポン・ドゥ・ヌムール・アンド・カンパニー オレフィンの重合方法
US6369194B1 (en) * 1998-11-09 2002-04-09 Yale University Vicinyl tricarbonyl compounds and combinatorial libraries containing same
JP2001055410A (ja) * 1999-06-08 2001-02-27 Denki Kagaku Kogyo Kk 重合用遷移金属触媒成分、それを用いた芳香族ビニル化合物−オレフィン共重合体及びその製造方法
JP4677671B2 (ja) * 1999-12-27 2011-04-27 東ソー株式会社 遷移金属化合物、オレフィン重合用触媒およびオレフィンの重合方法
JP2001181328A (ja) * 1999-12-27 2001-07-03 Mitsui Chemicals Inc オレフィン重合用触媒およびオレフィンの重合方法
US7259214B2 (en) * 2003-02-28 2007-08-21 The Regents Of The University Of California Metal catalyst for olefin polymerization and co-polymerization with functional monomers
US7589223B2 (en) * 2003-09-25 2009-09-15 Basell Polyolefine Gmbh Polymerization catalysts, preparation of polyolefins, organotransition metal compounds and ligands
US7205422B2 (en) * 2004-12-30 2007-04-17 Air Products And Chemicals, Inc. Volatile metal β-ketoiminate and metal β-diiminate complexes

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See references of EP2288626A4 *

Also Published As

Publication number Publication date
US8242297B2 (en) 2012-08-14
JP2011522071A (ja) 2011-07-28
CN102037025A (zh) 2011-04-27
CN102037025B (zh) 2012-10-10
EP2288626A4 (en) 2013-10-16
EP2288626A2 (en) 2011-03-02
JP5651107B2 (ja) 2015-01-07
US20090299020A1 (en) 2009-12-03
WO2009151825A3 (en) 2010-02-04

Similar Documents

Publication Publication Date Title
Coates et al. Catalysts for the living insertion polymerization of alkenes: access to new polyolefin architectures using Ziegler–Natta chemistry
Sacchi et al. Vinylic Polymerization of Norbornene by Late Transition Metal‐Based Catalysis
US20040158012A1 (en) Polymerization of olefinic compounds
JP5292059B2 (ja) α−オレフィン・(メタ)アクリル酸エステル共重合体の製造方法ならびにα−オレフィン・(メタ)アクリル酸エステル共重合体
CZ235197A3 (en) Alpha olefins, olefin polymers and process for preparing thereof
US20030130452A1 (en) Copolymers of ethylene with various norbornene derivatives
Liao et al. Regioselective polymerizations of α-olefins with an α-diamine nickel catalyst
JP5597582B2 (ja) 金属錯体ならびにそれを用いたα−オレフィン重合体の製造方法およびα−オレフィンと(メタ)アクリル酸エステル共重合体の製造方法
CN109400777B (zh) 基于苊醌双亚胺配体的钒配合物及其制备方法和应用
EP1188762A1 (en) Chromium complexes and their use for the polymerization of alpha-olefins
US8242297B2 (en) Transition metal initiators supported by ketone diimine ligands for the homopolymerization of olefins and the copolymerization of olefins with polar comonomers
Azoulay et al. Living polymerization of ethylene and α-olefins using a nickel α-keto-β-diimine initiator
JP2011088831A (ja) 新規な金属錯体ならびにそれを用いたα−オレフィン重合体の製造方法およびα−オレフィンとプロペン酸誘導体エステル共重合体の製造方法
Bao et al. Homo‐and copolymerization of norbornene with styrene catalyzed by a series of copper (II) complexes in the presence of methylaluminoxane
EP1068247A2 (en) Polymers of substituted cyclopentenes
Khoshsefat et al. Practical and theoretical study on the α-substituent effect on α-diimine Nickel (II) and Cobalt (II)-based catalysts for polymerization of ethylene
KR101165490B1 (ko) 새로운 전이금속 촉매, 및 이를 이용한 올레핀 중합방법
Zhao et al. Linear/branched block polyethylene produced by α-diimine nickel (II) catalyst and bis (phenoxy-imine) zirconium binary catalyst system in the presence of diethyl zinc
CN118994261A (zh) 含芳基取代的四氢萘酚-膦配合物及其制备方法与应用
Li et al. Synthesis and structural characterization of ethylene–norbornene copolymer with high norbornene content catalyzed by β-diketiminato nickel/methylaluminoxane
Saki Copolymerization of olefins with polar monomers by transition metal catalysts
WO2008033246A2 (en) Zwitterionic group viii transition metal initiators supported by olefin ligands
EP2104687A1 (en) Single component, phosphine-free, initiators for ethylene homopolymerization and copolymerization with functionalized co-monomers
CN118994260A (zh) 四氢萘酚-膦后过渡金属配合物及其制备方法和应用
Edson et al. Living Transition Metal‐Catalyzed Alkene Polymerization: Polyolefin Synthesis and New Polymer Architectures

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 200980118299.8

Country of ref document: CN

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 09763116

Country of ref document: EP

Kind code of ref document: A2

WWE Wipo information: entry into national phase

Ref document number: 2011510554

Country of ref document: JP

NENP Non-entry into the national phase

Ref country code: DE

REEP Request for entry into the european phase

Ref document number: 2009763116

Country of ref document: EP

WWE Wipo information: entry into national phase

Ref document number: 2009763116