WO1995012691A1 - Manufacture of silicon steel plate having excellent magnetic characteristic - Google Patents

Manufacture of silicon steel plate having excellent magnetic characteristic Download PDF

Info

Publication number
WO1995012691A1
WO1995012691A1 PCT/JP1994/001833 JP9401833W WO9512691A1 WO 1995012691 A1 WO1995012691 A1 WO 1995012691A1 JP 9401833 W JP9401833 W JP 9401833W WO 9512691 A1 WO9512691 A1 WO 9512691A1
Authority
WO
WIPO (PCT)
Prior art keywords
annealing
decarburization
steel sheet
silicon steel
texture
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP1994/001833
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
Toshiro Tomida
Shigeo Uenoya
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Corp
Original Assignee
Sumitomo Metal Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Metal Industries Ltd filed Critical Sumitomo Metal Industries Ltd
Publication of WO1995012691A1 publication Critical patent/WO1995012691A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01F—MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
    • H01F1/00—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties
    • H01F1/01—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials
    • H01F1/03—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity
    • H01F1/12—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials
    • H01F1/14—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials metals or alloys
    • H01F1/147—Alloys characterised by their composition
    • H01F1/14766—Fe-Si based alloys
    • H01F1/14775—Fe-Si based alloys in the form of sheets
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D3/00—Diffusion processes for extraction of non-metals; Furnaces therefor
    • C21D3/02—Extraction of non-metals
    • C21D3/04—Decarburising
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/12—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of articles with special electromagnetic properties
    • C21D8/1244—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of articles with special electromagnetic properties characterised by the heat treatment
    • C21D8/1255—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of articles with special electromagnetic properties characterised by the heat treatment with diffusion of elements, e.g. decarburising, nitriding
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D1/00—General methods or devices for heat treatment, e.g. annealing, hardening, quenching or tempering
    • C21D1/74—Methods of treatment in inert gas, controlled atmosphere, vacuum or pulverulent material
    • C21D1/773—Methods of treatment in inert gas, controlled atmosphere, vacuum or pulverulent material under reduced pressure or vacuum

Definitions

  • Patent application title Method for producing silicon steel sheet with excellent magnetic properties
  • the present invention relates to a method for producing a silicon steel sheet having a ⁇ 100 ⁇ plane parallel to a sheet surface and having excellent magnetic properties.
  • silicon steel sheets have been used as core materials for motors, generators, transformers, and the like.
  • This silicon steel sheet is required to have two characteristics: a small magnetic energy loss in an alternating magnetic field and a high magnetic flux density in a magnetic field. In order to realize these characteristics, it is effective to increase the electric resistance and integrate the ⁇ 100> axis of the bcc lattice, which is the direction of easy magnetization, in the direction of the used magnetic field.
  • a unidirectional silicon steel sheet containing about 3% of Si is often used as one exhibiting the most effective magnetic characteristics.
  • Figure 1 is a diagram schematically showing the rolling direction of silicon steel sheet and the accumulation orientation difference between the ⁇ 100> axis, the ⁇ 110> axis, and the ⁇ 100 ⁇ and ⁇ 110 ⁇ planes of the bcc lattice. It is.
  • the steel sheet shown in Fig. 1 (a) is a unidirectional silicon steel sheet with the ⁇ 110 ⁇ plane parallel to the sheet surface and the ⁇ 100> axis gathered in the rolling direction as shown in the figure. Since the easy magnetization direction of the silicon steel is the ⁇ 100> axis direction, this steel sheet has remarkably excellent magnetic properties when used by applying a magnetic field in the rolling direction. However, this unidirectional silicon steel sheet is hardly magnetized in directions other than the rolling direction. Therefore, when a magnetic field acts in various directions on the plate surface as in a rotating machine such as an electric motor or a generator, a desired effect cannot be obtained.
  • silicon is used in equipment where the magnetic field acts in multiple directions on the plate surface.
  • the raw steel sheet is a non-oriented silicon steel sheet having almost no texture.
  • silicon steel sheet since most ⁇ 100> axes are not parallel to the sheet surface, good magnetic properties cannot be obtained.
  • silicon steel sheets having these three types of textures are collectively referred to as silicon steel sheets having ⁇ 100 ⁇ plane texture.
  • ⁇ 100 ⁇ ⁇ 100> texture shown in Figs. 1 (b) and (c), or ⁇ ⁇ 100 ⁇ ⁇ 110> Texture is preferred.
  • the ⁇ 100 ⁇ plane shown in Fig. 1 (d) has a non-directional texture in the plate surface, or It is desirable that the ⁇ 100 ⁇ plane shown in (b) and (c) be textured in one direction on the plate surface ⁇ , punched out at different angles in the plate surface, and be used by overlapping.
  • the present inventors have disclosed in Japanese Patent Application Laid-Open No. 1-108345 a method for producing a silicon steel sheet using a two-stage decarburization annealing suitable for realizing such ⁇ 100 ⁇ plane texture on an industrial scale. showed that.
  • This production method contains C: 0.02 to 1%, Si: 0.2 to 6.5%, and, if necessary, removes Mn: 5% or less at least, and after decarburization, at substantially 850 ° C or less.
  • substantially becomes a single phase of a graphite means that a trace second phase such as MnS or A 1 N may be present.
  • vacuum or weak decarburization is used to generate Hi-ferrite grains having a ⁇ 100> axis in the direction perpendicular to the plate surface, essentially in a region 5 to 50 m deep from the surface.
  • Primary decarburization annealing in a neutral atmosphere eg, soaking temperature: 950 ° C, soaking time: 5 hours
  • a second decarburizing anneal in a strong decarburizing atmosphere for growth for example, soaking temperature: 850 ° C, soaking time: 2 hours is performed.
  • Fig. 2 is a diagram schematically showing the state of development of ⁇ 100 ⁇ texture on the plate surface.
  • the inside is a +7 two-phase coexisting structure, but the surface layer is a It shows the state where it is.
  • Process (1) above is caused by selective growth because the surface energy of the ⁇ 100 ⁇ orientation-ferrite crystal grains of the surface layer that has become a single phase of hypo-ferrite is smaller than those of other orientations. .
  • the driving force for selective growth by this surface energy is It is proportional to the ratio ( ⁇ E / d) between the difference in surface energy between ( ⁇ ) and the thickness of the surface layer (d). In other words, this driving force increases when the thickness of the surface layer that has become the single phase of the ferrite is small. Therefore, when the single phase of the filament is generated by annealing, the single phase of the single ferrite in the early stage of annealing is generated.
  • the ⁇ 100 ⁇ texture develops when the surface texture becomes thin. In other words, in order to develop the ⁇ 100 ⁇ texture, the surface layer that quickly became a single phase of ferrite in the early stage of annealing was formed, and the thickness of this surface layer was sufficient for the development of the texture. It is necessary to control decarburization and Mn so that the thickness does not increase. In addition, if the boundary between the surface layer and the inside of this single ferrite single phase is not clear, the ⁇ 100 ⁇ crystal grains in the surface layer will not grow efficiently.
  • an open coil method is used as the first decarburizing annealing, and an open coil method or a continuous annealing method is used as the second decarburizing annealing.
  • the open coil method there is a quality problem that the steel plate buckles during annealing.
  • primary annealing is performed at a high temperature of 900 or more, so that buckling is liable to occur, especially for long ones.
  • the continuous annealing method has a problem that the annealing furnace is long and the equipment cost increases because the annealing is performed for a relatively long time. Given these problems, conventional manufacturing methods are not efficient in terms of productivity, manufacturing cost and quality.
  • the primary annealing atmosphere has only a very weak decarburizing effect, it cannot be used as the secondary annealing atmosphere, and in the strong decarburizing atmosphere of the secondary annealing, Si and Mn in the steel sheet cannot be used. Since it is strongly oxidized to form a surface oxide layer, if this is used as a primary annealing atmosphere, the ⁇ 100 ⁇ plane texture does not develop. Is this a problem? Therefore, it is indispensable to adopt a two-stage annealing method of primary and secondary decarburization annealing. Disclosure of the invention
  • An object of the present invention is to solve the conventional problems described above and to provide a method capable of manufacturing a silicon steel sheet having a ⁇ 100 ⁇ plane texture by a single annealing.
  • the present inventors have found that a substance that promotes decarburization, or a substance that promotes decarburization and a substance that promotes Mn removal are sandwiched between coil layers or between sheets as an annealing separation material and subjected to annealing in a single annealing In addition to causing the ⁇ -> transformation, a ⁇ 100 ⁇ plane parallel to the plate surface is formed, and the ferrite grains grow toward the center of the plate. 0 0> It was found that a shaft could be formed, and the production method of the present invention was completed. Moreover, according to this manufacturing method, even a long steel plate can be manufactured while preventing buckling.
  • the gist of the present invention is that the following ⁇ S> 0
  • a cold rolled silicon steel sheet having the above composition is subjected to tight coil annealing or multi-layer annealing using a substance that promotes decarburization and a substance that promotes demanganese as an annealing separator. Production method.
  • Figure 1 shows the rolling direction of silicon steel sheet and the ⁇ 100> axis of the bcc lattice
  • Fig. 2 shows the state of development of ⁇ 100 ⁇ texture on the plate surface. It is the figure which showed typically.
  • Fig. 3 is a diagram showing the structure of the laminate used in the annealing test
  • Fig. 4 is a schematic diagram showing the concentration distribution of C and Mn due to diffusion when a steel sheet is annealed.
  • FIGS. 5 and 6 are schematic views of microstructures when materials having different Mn are annealed using both the decarburization promoting material and the Mn promoting material.
  • Fig. 5 shows the case where a silicon steel sheet containing 0.92% Mn was annealed
  • Fig. 6 shows the case where a silicon steel sheet containing no Mn was annealed.
  • FIG. 7 is a diagram showing the chemical compositions of nine kinds of ingots manufactured by vacuum fabrication as the test materials of Examples 1 to 4.
  • FIG. 8 shows the decarburizing annealing conditions and properties after annealing in Example 1
  • Fig. 9 shows the conditions of the annealing separator, C content and magnetic properties after annealing in Example 2
  • Fig. 10 shows the decarburizing properties in Example 3. It is a figure which shows the carbon annealing conditions, the C content after annealing, and magnetic characteristics, respectively.
  • Fig. 11 is a graph showing the effect of annealing time on the contents of carbon and Mn in Example 4.
  • Fig. 12 shows 18 types of specimens manufactured by vacuum forming as test materials of Examples 5 to 8.
  • FIG. 2 is a view showing a chemical composition of the ingot of FIG.
  • Fig. 13 shows the Mn content, C content, ⁇ 100> axial density and magnetic properties after decarburizing annealing in Example 5, and Fig. 14 shows the Mn content, C content and It is a figure which shows ⁇ 100> axis density.
  • Figure 15 is a pole figure showing the formation of a sharp ⁇ 100 ⁇ ⁇ 052> texture.
  • Figure 16 shows the relationship between the rolling direction of the material, the magnetic flux density and the iron loss value.
  • FIG. 17 shows the comparison of the magnetization curve of the sample in Example 8 with the comparison material (commercially non-directional FIG. 18 is a diagram showing the magnetization curve of the magnetic steel sheet S-9), and FIG. 18 is a diagram showing the Mn content, C content, ⁇ 100> axis density, and magnetic properties after annealing.
  • decarburization occurs while preventing oxidation of the steel sheet surface.
  • a strong ⁇ 1 ⁇ o ⁇ plane texture develops on the surface by the transformation. This decarburization reaction is sufficiently fast for practical use.
  • a crystal with ⁇ 100 ⁇ plane texture grows inside the plate within the practical annealing time, and the entire plate Can be made of ⁇ 100 ⁇ plane texture.
  • Si0 2 oxides of Si
  • Decarburization promoting action in the case of using Si0 2 as an annealing separator material is estimated to be due to the following mechanism.
  • the oxide of Si is stable at room temperature, but becomes unstable at a temperature of about 1000 ° C.
  • the decarburization reaction of equation (2) occurs strongly at the contact point between the oxide and the steel sheet. And 1 generated by the formula The oxygen does not react with the carbon in the steel sheet after being changed to oxygen gas (02), but remains in the state of oxygen (0) as shown in equation ( 2 ), and reacts with the carbon on the steel sheet surface in direct contact. Responding.
  • the reactions (1) and (2) above have a strong solid-state reaction.
  • the substance having an action as described above, other Cr 2 0 3, FeO, is a relatively unstable oxides in a high temperature suitable atmosphere, such as Na 2 C0 3.
  • a high temperature suitable atmosphere such as Na 2 C0 3.
  • it is a substance that decomposes at the annealing temperature to generate oxygen and promotes decarburization, or a substance containing these substances.
  • These can be used as a mixture of two or more.
  • Na 2 C0 3 is unstable as compared with Si0 2, because fast degradation rate at high temperatures, to generate a large amount of oxygen, Si in the steel sheet, to oxidize the Mn, causes surface oxidation of the steel sheet.
  • Na 2 C0 3 shall limit or avoid alone or mixed amount.
  • Si0 2 from the viewpoint of the decomposition temperature and the oxygen generation amount, so to accelerate the decarburization without causing surface oxidation of the steel sheet, the optimal substance that promotes the development of ⁇ 100 ⁇ plane texture.
  • Oxygen (0) generated from the decarburization promoting material oxidizes Mn in the steel sheet and deteriorates surface appearance. Therefore, in the case of a steel sheet containing Mn, if a material that promotes de-Mn is used in combination with a decarburization-promoting material, Mn, which is a stabilizing element, is reduced from the surface layer of the steel sheet, so that the transformation from 7 to e is promoted, Also suppresses oxidation of Mn. Mn that is not oxidized activates the surface of the steel sheet and promotes the decarburization reaction according to the above formula (1). Furthermore, de-Mn can be applied to promote the 7 ⁇ transformation on the surface.
  • the form of the annealing separator containing a substance that promotes decarburization is not particularly limited.
  • This The form may be a plate or a powder, a fibrous form thereof or a sheet form made of a woven fabric, or a mixture of the sheet and the powder. Most preferred is a fibrous or woven sheet.
  • the reason is that unlike the powder, there is no dropout between the coil layers and a large amount of adsorbed oxygen on the surface, and the voids existing between the fibers make it easy for the carbon monoxide generated by the above reaction to be discharged out of the coil. And sublimation of Mn in the voids to promote the ⁇ ⁇ transformation on the surface. These can be easily sandwiched between coil layers or between plates.
  • FIG. 3 is a diagram showing the configuration of the laminate used in the annealing test.
  • 1 is a laminated body
  • 2 is a test plate
  • 3 is a Mn removal promoting material
  • 4 is a decarburization promoting material.
  • a test plate 2 Mn-containing silicon steel plate
  • a steel plate 3 for promoting Mn removal a material containing no Mn, that is, a material that promotes Mn removal
  • a decarburization promoting material 4 as an annealing separator.
  • Mn sublimated from the test plate passes through the decarburization promoting material as indicated by the arrow L in the figure and is absorbed by the steel plate for promoting Mn removal.
  • Such a reaction is due to the fact that a large amount of Mn is present in the steel sheet for promoting Mn removal after annealing. It is also confirmed from the fact that the amount of de-Mn in the test plate is larger than in the case where annealing is performed using only the decarburization promoting material without using the steel sheet for promoting Mn removal.
  • the promotion of Mn removal in this manner is the first step of forming the ⁇ 100 ⁇ texture described above (7 ⁇ transformation occurs at the surface layer, and the ⁇ 100 ⁇ crystal grains are generated by surface energy within the surface layer. Selective growth promotes the ⁇ 100 ⁇ texture in the lateral direction).
  • the substance that promotes Mn removal is an iron-based alloy containing no Mn, or an iron-based alloy or Mn containing Mn less than the Mn content of the silicon steel sheet (preferably 1/2 or less of the Mn content of the silicon steel sheet).
  • oxide that absorbs e.g., oxide forming a Mn composite compound, T i 0 2
  • any substance that absorbs Mn sublimated from the steel sheet during annealing and does not adversely affect the decarburization reaction or the surface energy state of the steel sheet may be used.
  • the shape may be powdery, fibrous, plate-like or the like, and is not particularly limited. It is preferable that the Mn content of the iron-based alloy be less than or equal to 1/2 of the Mn content of the silicon steel sheet, and the other components be equal.
  • T i 0 2 oxides that promote de-Mn forms Mn composite oxide which sublimes from steel plate (T i Mn0 2), to absorb Mn.
  • the oxide that promotes Mn removal can be used in an annealing separator for promoting decarburization, and decarburization annealing can be performed more effectively than with an iron-based alloy sheet.
  • Fig. 4 is a schematic diagram showing the concentration distribution of C and Mn due to diffusion when a steel sheet is annealed.
  • C shows the concentration distribution when only decarburization is performed
  • Mn shows the concentration distribution when Mn is removed. I have.
  • annealing is performed at around 1 000 ° C and only decarburization proceeds, such a carbon concentration distribution is formed.However, since the diffusion rate of carbon is extremely large, the difference in carbon concentration between the surface and the inside is small.
  • Single-flight single-phase surface structure is not formed or formed However, the boundary between the surface structure (the structure that became a single phase of ferrite) and the internal structure (the structure of +7 or 7) becomes unclear, and the thickness of the surface structure increases. 100 ⁇ The texture cannot be fully developed.
  • the diffusion rate of Mn is much smaller than that of carbon, as shown in Fig. 4, and a large concentration gradient near the surface due to de-Mn (low Mn surface layer and high Mn internal Can form a low Mn region.
  • the carbon in the region (low-Mn surface layer) diffuses into the high-Mn region (inside the plate), and a 7 ⁇ transformation occurs in that region, and the region is converted to a single-fluorine single crystal. Phase.
  • the surface layer formed by removing Mn does not become too thick even after prolonged annealing because of the low diffusion rate of Mn (about 100 zm even at 1000 ° C for 12 hours). Therefore, if the decarburization promoting material and the Mn promoting material are used together and annealed (1000 ° C, 12h), the ferrite single phase is initially formed on the extreme surface layer (from 20 zm to 70 m) due to the Mn removal. The surface layer is formed, and if decarburization proceeds sufficiently later, this surface layer grows inward. Keeping the surface texture of the well-defined single phase of the phase thin allows the ⁇ 100 ⁇ crystal grains to grow due to surface energy, and the ⁇ 100 ⁇ texture to grow strongly.
  • FIG. 5 and FIG. 6 are schematic views of microstructures when materials having different Mn obtained in examples described later are annealed using both a decarburization promoting material and a Mn removing promoting material.
  • (A) to (e) in Fig. 5 show changes in the microstructure of a silicon steel sheet containing 0.92% Mn (steel type 0 in Fig. 12 described later) depending on the annealing time. Due to the effect of de-Mn, a clear single ferrite single-phase region exists near the surface of the steel sheet when the annealing time is within 1 hour [(a) and (b)].
  • FIG. 6 show changes in the microstructure of the silicon steel sheet containing no Mn (steel type 0-M in FIG. 12 described later) depending on the annealing time. Since there is no Mn removal effect in steels containing no Mn, a clear surface layer is not formed, decarburization proceeds uniformly over the entire plate thickness, and grain growth occurs almost in the vicinity of and inside the plate surface. .
  • the cold-rolled steel sheet to which a substance that promotes decarburization or Mn removal is applied as an annealing separator may be either a coiled sheet or a cut sheet.
  • the former case corresponds to tight coil annealing, and the latter case corresponds to laminar annealing.
  • the cold-rolled steel sheet is coiled and a sheet-like annealed material is used in actual operation, it is better to overlap the cold-rolled steel sheet and wind it into a coil.
  • oxide powder When applying oxide powder to a cold-rolled steel sheet, it can be applied before winding by a winding device.
  • a long steel plate without buckling can be manufactured by tight coil annealing using such an annealing separator.
  • the annealing atmosphere is mainly composed of hydrogen, inert gas, or a mixture of both. Atmosphere or vacuum. Preferred is a vacuum of less than 100 Torr, more preferred is a vacuum of less than 1 Torr. If the atmospheric pressure exceeds 100 Torr, the desired oxygen separation reaction, decarburization reaction, and ⁇ 100 ⁇ plane texture with a high degree of accumulation are unlikely to occur.
  • the holding temperature is desirably 1300 ° C or less. Annealing temperatures exceeding 1300 ° C are difficult to achieve industrially. It is preferable to use a +7 two-phase coexistence temperature range or a temperature range of 850 ° C. or higher in order to obtain a ⁇ 100 ⁇ plane texture with high integration.
  • the soaking time for annealing is preferably in the range of 30 minutes to 100 hours. If it is less than 30 minutes, decarburization or Mn removal will be insufficient. On the other hand, if it exceeds 100 hours, productivity will deteriorate.
  • Chemical composition of cold rolled silicon steel sheet :
  • the C content is 1% in the steel sheet before decarburization annealing. It is necessary to: The lower the content of C, the better.
  • the preferred upper limit of the C content is 0.5%, and the more preferred is 0.2%.
  • the content be 0.01% or more. In this way, at the stage after annealing.
  • the content is preferably less than 0.01%, preferably not more than 0.055%, more preferably not more than 0.003% so as not to deteriorate the magnetic properties. This is because the remaining carbon precipitates as cementite in the free light and deteriorates the magnetic properties.
  • Si To ensure magnetic and mechanical properties, a Si content of 0.2% or more is required. Preferred is 1% or more. On the other hand, the upper limit of the Si content is set to 6.5% in order to suppress embrittlement and a decrease in magnetic flux density. Preferred is 5% or less, more preferred is 4% or less.
  • the Mn can be increased, but the Mn content should not exceed 5% in order to reduce the magnetic flux density.
  • an annealing separator consisting of a decarburization promoting material and a decarburization promoting material and a Mn removal promoting material is sandwiched between the layers of the coil or between the sheets.
  • the density of the annealing separator can be selected so that excessive oxygen is not supplied.
  • the density of the annealed separator is indicated by the mass per unit area, and in the case of a sheet, it is proportional to the thickness. Further, since the amount of generated oxygen changes depending on the annealing temperature, it can be controlled also by this temperature. Oxidation of the steel sheet surface can be sufficiently prevented by such controlled filling of the annealing separator and supply of oxygen.
  • decarburization promoting material is an oxide such as Si0 2
  • the decomposition of Si0 2 when the oxygen amount is increased does not occur. That is, the oxygen decomposition reaction of the above formula (1) stops or proceeds in the opposite direction, and the increase in the amount of oxygen stops or conversely decreases. This reaction is automatically controlled so that Si in the steel sheet is not oxidized.
  • the oxidation potential of Mn is very close to that of Si, so there is an effect that Mn is not oxidized.
  • the production of silicon steel sheets usually involves the steps of continuous production, hot working and cold rolling.
  • cold rolling any rolling method can be used as long as cold rolling is performed at a rolling reduction of 10% or more.
  • the preferred reduction is 30% or more, and the more preferred reduction is 50% or more. In this case, it does not prevent one or more annealings from being inserted between the hot working and the subsequent working.
  • cold rolling refers to rolling at 500 ° C or lower where recrystallization does not occur.
  • the sheet thickness after cold rolling is preferably 5 rara or less. If the plate thickness exceeds 5 ram, it takes a long time to decarburize the inside and the eddy current loss increases. Preferred is 1 mra or less, and more preferred is 0.5 mm or less. — On the other hand, the lower limit of the sheet thickness is not particularly limited as long as it can be manufactured by cold rolling.
  • Figure 7 is a diagram showing the chemical composition of nine types of ingots manufactured by vacuum forging. These ingots were hot forged into l Orara-thick steel sheets, and each steel sheet was replaced with 3 ingots. After hot rolling to a thickness of 1 mm, cold rolling was performed to a thickness of 1 mra. Five 250-mra square test plates were cut from each of these cold-rolled steel plates and used as test materials for simulating tight coil annealing.
  • the X-ray integrated intensity was measured at the position of 2Z5 of the plate thickness from the surface of each test plate after the decarburization annealing, and ⁇ 100> in the direction perpendicular to the plate surface was determined from the integrated intensity of the ⁇ 200 ⁇ surface reflection. > The axial density was determined as a multiple of the sample without orientation. For comparison, the same measurement was performed on a comparative example and a commercially available high-grade non-oriented silicon steel sheet having a thickness of 0.5 mra ( ⁇ HSS-9).
  • FIG. 8 is a diagram showing decarburization annealing conditions and measurement results of properties after annealing. At this time, the same measurement was performed by alternately laminating the 0-M steel and the de-Mn promoting material in Fig. 12 described later through the decarburizing promoting material, and the same results were obtained. It was shown to.
  • a hot-rolled steel sheet having a thickness of 3 mm of steel I shown in FIG. 7 was cold-rolled into a steel sheet having a thickness of 0.35 mra, and a 200-mni square test plate was cut out from the obtained steel plate.
  • Each five to sandwich the decarburization promotion laminate as annealing separator material between the panels for testing, in a vacuum of 0. l kg / cm 2 in surface pressure was added l T orr the laminate of 1050 ° C x 24 hours Decarburization annealing was performed.
  • the ten ring yield test specimens were laminated, and the primary and secondary coils were wound around this for 100 turns, and the magnetic properties were measured.
  • the same measurement was performed on a comparative material and a commercially available high-grade non-oriented silicon steel sheet having a thickness of 0.35 (JIS S-9).
  • FIG. 9 is a diagram showing the conditions of the annealing separator, the C content after annealing, and the measurement results of the magnetic properties.
  • the hot-rolled steel sheet of G steel shown in Fig. 7 with a reference thickness of 4 is cold-rolled to a thickness of 2 mm, then subjected to intermediate annealing at 900 ° C for 3 minutes, and then cold-rolled to 0.35 rara.
  • a 200 mra square test plate was cut out from the obtained steel plate.
  • Example 2 The same evaluation test as in Example 2 was performed on the test plate after the decarburization annealing.
  • FIG. 10 is a diagram showing decarburizing annealing conditions (including vacuum conditions), C content after annealing, and measurement results of magnetic properties.
  • the method of the present invention shows that the amount of carbon is reduced by a single annealing, and that excellent magnetic properties are obtained.
  • Example 2 a 200-rara square test plate was cut out from a steel plate obtained by cold rolling the steel B shown in FIG. 7 to a recommended thickness of 0.35.
  • As the annealing separator material between the five panels for testing 50 wt% A1 2 0 3 - scissors 50 wt% Si0 2 system decarburization promoting material fibrous density of 25rag / cm 2, Example 2
  • decarburization annealing was performed at 975 ° C for about 20 hours. Carbon and Mn were analyzed for the test plate during this decarburization annealing.
  • FIG. 11 is a diagram showing the effect of annealing time on the contents of carbon and Mn. As shown in the figure, it can be seen that in the method of the present invention, decarburization and Mn removal are performed efficiently.
  • Figure 12 is a diagram showing the chemical composition of 18 types of ingots manufactured by vacuum forging.These ingots were hot forged into 50 mm thick steel plates, and each steel plate was further thickened three times. After hot rolling, it was cold rolled to a thickness of 0.35 mm.
  • the steel with H added after the steel type symbol in the comparative example is a steel containing no carbon, and has almost the same composition as the steel without H, except for the carbon content.
  • Stepel 0-M does not contain Mn It is a steel and used as a steel sheet for promoting Mn removal.
  • test plates Five 400 mm square test plates were cut out of each of these cold-rolled steel plates, and used as test materials for simulating tight coil annealing.
  • this weave-like decarburizing accelerator is close to the composition of an oxide called mullite, and most of it is amorphous or mullite formed by X-ray diffraction. It is known to have a crystalline structure. After being used as an annealed separator, in most cases it was a mixture of mullite and a small amount of christ barite.
  • Figure 13 shows the Mn content, C content, ⁇ 100> axial density, and magnetic properties after decarburization annealing.
  • () indicates the steel sheet for promoting Mn removal. Indicates the value when is not used.
  • test sheets 70 wt% A1 2 0 3 - 30 wt% Si0 particle size 2 system decarburization promoting material fibrous 10 to 50 m of the Ti0 2 powder of which was added various amounts 0.01 g /
  • the laminate was sandwiched at a density of 2 cm 2, a surface pressure of 0.2 kg / cm 2 was applied to the laminate, and annealing was performed at 1050 ° C for 6 hours in a vacuum of lO- 'Torr. The heating rate was 1 mm.
  • the ⁇ 100> axis density and the contents of carbon and Mn were analyzed in the same manner as in Example 5.
  • the thickness of the test sheets and Ti0 2 charge ⁇ further Mn content after annealing is a diagram showing the C content and ⁇ 1 0 0> axis density, as kana bright et From this result , Ti0 2 de Mn is promoted by the use of powder, it can be seen that to develop stronger ⁇ 100 ⁇ plane texture.
  • FIG. 15 is a ⁇ 110 ⁇ pole figure showing the formation of a strong ⁇ 100 ⁇ ⁇ 052> texture
  • FIG. 14 shows the texture of the sample after annealing shown in No. 3 in FIG. Measured using 110 reflection of Hi-Fe by Co-K line.
  • 1 1 0> axis density is very large in 8 directions inclined 45 ° from the vertical direction of the sheet surface, and this material has strong ⁇ 100 ⁇ texture
  • the ⁇ 100 ⁇ texture has ⁇ 100 ⁇ ⁇ 052> type plane anisotropy.
  • FIG. 16 is a diagram showing the relationship between the rolling direction of the material and the magnetic flux density (a) and the iron loss value (b). These relationships are as follows: a strip sample of 3 cm in width and 10 cm in length is cut out from the annealed material shown in No. 3 in Fig. 14 so that the longitudinal direction is in various rolling directions, and magnetic flux density at a magnetizing force of lOOOA / m to (B 1 ()) and iron loss (W 1 5 / 5.) was determined by single-plate magnetization measurement device.
  • a vacuum-melted ingot having a composition indicated by steel type N in FIG. 12 was formed into a plate having a thickness of 30 mra by hot forging, and each plate was hot-rolled to a thickness of 3 mm. After annealing for one minute, it was cold rolled to a thickness of 0.5 band.
  • Thailand Tokoiru annealing to Shiyu Mi rate cut out panels for testing of 400 ⁇ from the cold-rolled sheet, annealing separator material as 20 wt% A1 2 0 3 - 80 wt% Si0 2 system fibrous decarburization
  • the accelerating material is filled at a density of 0.005 g / cra 2 , and Si0 2 and Ti0 2 powder with a diameter of 100 / zm are sandwiched between test plates at a density of 3 mg / cra 2 each, and laminated. Applied a surface pressure of 0.2 kg / cm 2 .
  • Ten-ring-shaped test pieces were laminated, to which the primary coil, 100 turns Dzu' winding the secondary coil, the magnetic flux density when applying an external magnetic field of 1000A / m, and 5000A / m (B,., And B 5 ), And iron loss when magnetized to a magnetic flux density of 1 T (tesla) and 1.5 T in an alternating magnetic field of 50 Hz (
  • Fig. 17 shows the magnetization curve of the sample together with the magnetization curve of the comparative material (commercially non-oriented electrical steel sheet S-9).
  • Fig. 18 shows the Mn content, C content, and ⁇ 100 It is a figure which shows axial density and magnetic characteristics. From all the results, it can be seen that superior magnetic properties are obtained with the material of the present invention as compared with the comparative material. Industrial applicability
  • a silicon steel sheet having excellent magnetic properties and a high degree of ⁇ 100 ⁇ plane integration can be efficiently produced by a single tight coil annealing or multilayer annealing.
  • annealing is performed by tight coil annealing or laminated annealing using an annealing separation material, buckling of the steel sheet is eliminated and a long material can be manufactured, so that it can be used in the field of manufacturing a steel sheet.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Physics & Mathematics (AREA)
  • Materials Engineering (AREA)
  • Thermal Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Mechanical Engineering (AREA)
  • Electromagnetism (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Dispersion Chemistry (AREA)
  • Power Engineering (AREA)
  • Manufacturing & Machinery (AREA)
  • Soft Magnetic Materials (AREA)
  • Manufacturing Of Steel Electrode Plates (AREA)
PCT/JP1994/001833 1993-11-02 1994-10-31 Manufacture of silicon steel plate having excellent magnetic characteristic Ceased WO1995012691A1 (en)

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP5/274373 1993-11-02
JP27437393 1993-11-02
JP6/249401 1994-10-14
JP24940194A JP3480072B2 (ja) 1993-11-02 1994-10-14 磁気特性の優れた珪素鋼板の製造方法

Publications (1)

Publication Number Publication Date
WO1995012691A1 true WO1995012691A1 (en) 1995-05-11

Family

ID=26539267

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP1994/001833 Ceased WO1995012691A1 (en) 1993-11-02 1994-10-31 Manufacture of silicon steel plate having excellent magnetic characteristic

Country Status (2)

Country Link
JP (1) JP3480072B2 (enExample)
WO (1) WO1995012691A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0741191A3 (en) * 1995-05-02 1997-10-29 Sumitomo Metal Ind Electrical sheet with improved magnetic properties and improved punchability

Families Citing this family (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1998020179A1 (fr) * 1996-11-01 1998-05-14 Sumitomo Metal Industries, Ltd. Plaque d'acier electromagnetique bidirectionnelle et procede de fabrication de cette derniere
TW476790B (en) * 1998-05-18 2002-02-21 Kawasaki Steel Co Electrical sheet of excellent magnetic characteristics and its manufacturing method
MX366630B (es) 2011-04-27 2019-07-17 Nippon Steel Corp Star Láminas de metal a base de fierro y método para fabricar las mismas.
CN109563583B (zh) 2016-08-05 2021-10-15 日本制铁株式会社 无方向性电磁钢板、无方向性电磁钢板的制造方法及马达铁芯的制造方法

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS4832722A (enExample) * 1971-09-02 1973-05-02
JPS552751A (en) * 1978-06-21 1980-01-10 Nippon Steel Corp Manufacture of one-way type electromagnetic steel sheet
JPS59205420A (ja) * 1983-05-02 1984-11-21 Kawasaki Steel Corp 一方向性珪素鋼板の製造方法
JPH01108345A (ja) * 1987-10-19 1989-04-25 Sumitomo Metal Ind Ltd 磁気特性の優れた珪素鋼板およびその製造方法
JPH02274844A (ja) * 1989-04-18 1990-11-09 Sumitomo Metal Ind Ltd 磁気特性の優れた電磁鋼板及びその製造方法

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS4832722A (enExample) * 1971-09-02 1973-05-02
JPS552751A (en) * 1978-06-21 1980-01-10 Nippon Steel Corp Manufacture of one-way type electromagnetic steel sheet
JPS59205420A (ja) * 1983-05-02 1984-11-21 Kawasaki Steel Corp 一方向性珪素鋼板の製造方法
JPH01108345A (ja) * 1987-10-19 1989-04-25 Sumitomo Metal Ind Ltd 磁気特性の優れた珪素鋼板およびその製造方法
JPH02274844A (ja) * 1989-04-18 1990-11-09 Sumitomo Metal Ind Ltd 磁気特性の優れた電磁鋼板及びその製造方法

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0741191A3 (en) * 1995-05-02 1997-10-29 Sumitomo Metal Ind Electrical sheet with improved magnetic properties and improved punchability
US5714017A (en) * 1995-05-02 1998-02-03 Sumitomo Metal Industries, Ltd. Magnetic steel sheet having excellent magnetic characteristics and blanking performance

Also Published As

Publication number Publication date
JPH07173542A (ja) 1995-07-11
JP3480072B2 (ja) 2003-12-15

Similar Documents

Publication Publication Date Title
RU2092605C1 (ru) Листы изотропной электротехнической стали и способы их изготовления
KR100224283B1 (ko) 자기특성과 타발성이 우수한 전자강판
JP7133708B2 (ja) 方向性電磁鋼板用焼鈍分離剤組成物、方向性電磁鋼板および方向性電磁鋼板の製造方法
CN113166872B (zh) 双取向电工钢板及其制造方法
JP2535963B2 (ja) 磁気特性の優れた珪素鋼板およびその製造方法
US3351501A (en) Process for producing magnetic sheets with cube-on-face grain texture
EP0906963B1 (en) Bidirectional electromagnetic steel plate and method of manufacturing the same
JP2001247944A (ja) 低磁歪二方向性電磁鋼板およびその製造方法
CN100545960C (zh) 磁芯以及使用该磁芯的应用产品
US5807441A (en) Method of manufacturing a silicon steel sheet having improved magnetic characteristics
JP2015061941A (ja) 優れた磁気特性を有するFe系金属板
JP3480072B2 (ja) 磁気特性の優れた珪素鋼板の製造方法
JPH01252727A (ja) 二方向性珪素鋼板およびその製造方法
EP1116798B1 (en) Hot rolled electrical steel sheet excellent in magnetic characteristics and corrosion resistance and method for production thereof
JP2576621B2 (ja) 磁気特性の優れた珪素鋼板
JP2590533B2 (ja) 珪素鋼板の製造方法
JPH02274844A (ja) 磁気特性の優れた電磁鋼板及びその製造方法
KR950013285B1 (ko) 고투자율 자성 박강판의 제조방법
JP4300661B2 (ja) 磁気特性に優れる二方向性珪素鋼板の製造方法
JP2016183358A (ja) 高強度、高磁束密度のFe系金属板及びその製造方法
JP2009007642A (ja) {100}集合組織珪素鋼板の製造方法
JPH04202644A (ja) 電磁鋼板およびその製造方法
JP2001158914A (ja) 二方向性珪素鋼板の製造方法
JPH0623411B2 (ja) 異方性の小さい電磁鋼板の製造方法
JP2015010241A (ja) Fe系金属板及びその製造方法

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): US

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE

ENP Entry into the national phase

Ref country code: US

Ref document number: 1995 464639

Date of ref document: 19950620

Kind code of ref document: A

Format of ref document f/p: F

121 Ep: the epo has been informed by wipo that ep was designated in this application
122 Ep: pct application non-entry in european phase
ENP Entry into the national phase

Ref country code: US

Ref document number: 1996 732894

Date of ref document: 19961017

Kind code of ref document: A

Format of ref document f/p: F