WO1995003349A1 - Heat-resistant water-dispersible sulfopolyester compositions - Google Patents

Heat-resistant water-dispersible sulfopolyester compositions Download PDF

Info

Publication number
WO1995003349A1
WO1995003349A1 PCT/US1994/007850 US9407850W WO9503349A1 WO 1995003349 A1 WO1995003349 A1 WO 1995003349A1 US 9407850 W US9407850 W US 9407850W WO 9503349 A1 WO9503349 A1 WO 9503349A1
Authority
WO
WIPO (PCT)
Prior art keywords
mole percent
naphthalene
dicarboxylic acid
diol
sulfopolyester
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US1994/007850
Other languages
English (en)
French (fr)
Inventor
Scott Ellery George
Bobby Jones Sublett
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Eastman Chemical Co
Original Assignee
Eastman Chemical Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Family has litigation
First worldwide family litigation filed litigation Critical https://patents.darts-ip.com/?family=22252150&utm_source=google_patent&utm_medium=platform_link&utm_campaign=public_patent_search&patent=WO1995003349(A1) "Global patent litigation dataset” by Darts-ip is licensed under a Creative Commons Attribution 4.0 International License.
Application filed by Eastman Chemical Co filed Critical Eastman Chemical Co
Priority to JP50520195A priority Critical patent/JP3369566B2/ja
Priority to CA002166543A priority patent/CA2166543C/en
Priority to EP94922540A priority patent/EP0710259B1/en
Priority to DE69413694T priority patent/DE69413694T2/de
Publication of WO1995003349A1 publication Critical patent/WO1995003349A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G63/00—Macromolecular compounds obtained by reactions forming a carboxylic ester link in the main chain of the macromolecule
    • C08G63/68—Polyesters containing atoms other than carbon, hydrogen and oxygen
    • C08G63/688—Polyesters containing atoms other than carbon, hydrogen and oxygen containing sulfur
    • C08G63/6884—Polyesters containing atoms other than carbon, hydrogen and oxygen containing sulfur derived from polycarboxylic acids and polyhydroxy compounds
    • C08G63/6886—Dicarboxylic acids and dihydroxy compounds

Definitions

  • the present invention relates to sulfonate
  • the sulfopolyesters utilize at least two dicarboxylic acids, one of which is a naphthalene dicarboxylic acid. This combination of dicarboxylic acids allows for the sulfopolyesters to maintain glass transition temperatures (Tg) of greater than 89°C. and exhibit lower melt viscosities than sulfopolyesters containing all naphthalenediyl units or all isophthtaloyl units.
  • Tg glass transition temperatures
  • the sulfopolyesters of this invention are useful in applications where improved heat and blocking resistance is required.
  • U.S. Pat. Nos. 3,546,008, 3,563,942, 3,734,874, and 3,779,993 disclose water-dispersible copolyester and polyesteramide compositions containing metal sulfonate groups. None of the references, however, use poly(ethylene-2,6-naphthalene
  • wate- dispersible or water-dissipatible .
  • compositions contain 1 to 5 mole% of 5-sulfoisophthalic acid with 75 mole% of the total acid component comprised of 2,6 or
  • Improved hydrolytic stability was advocated as an attribute of the invention.
  • the polyesters are less likely to be water dispersible.
  • Water-dispersible sulfopolyesters containing only isophthalate acid units or only terephthalic acid units tend to have Tg's less than 89°C. with aliphatic and alicyclic diols, while analogous systems containing only naphthalene dicarboxylic acid units tend to have a maximum Tg around 130°C., when common aliphatic and cycloaliphatic diols are used.
  • the present inventors have determined that sulfopolyesters based on isophthalate or terephthalate units modified with naphthalene units not only maintain Tg's in the
  • isophthalic acid or only naphthalene dicarboxylate units It is desirable to have lower melt viscosities. Since production process equipment is limited to a certain melt viscosity. Thus, lower melt viscosities will allow for higher molecular weights to be obtained for a given sulfopolyester.
  • Still another object of the invention is to provide water-dispersible sulfopolyester compositions which are useful in applications where increased abrasion
  • a water-dispersible sulfopolyester having a Tg of greater than 89°C. and low melt viscosity consisting essentially of repeat units from:
  • a dicarboxylic acid selected from the group consisting of aromatic dicarboxylic acids, saturated aliphatic dicarboxylic acids, cycloaliphatic dicarboxylic acids, and combinations thereof;
  • dicarboxylic acid and 100 mole percent diol.
  • This invention discloses compositions and methods of preparation for linear, water-dispersible
  • water-dispersible is used interchangeably with other descriptors such as “water-dissipatible”, “water-soluble”, or
  • water-dispellable All of these terms refer to the activity of water or a mixture of water with a
  • the sulfopolyester contains repeat units from at least two dicarboxylic acids, a diol, and a difunctional sulfomonomer. At least one of the dicarboxylic acids, component (a), is 10 to 93 mole percent based on 100 mole% dicarboxylic acid component, of naphthalene-2,6-dicarboxylic acid, naphthalene-2,7-dicarboxylic acid, naphthalene-2,6-dicarboxylate ester, or
  • naphthalene-2,7-dicarboxylate ester Preferably, the dimethyl ester forms are used.
  • the dicarboxylic acid component contains 2 to 85 mole percent of a dicarboxylic acid, component (b), which is selected from aliphatic, alicyclic, and aromatic
  • dicarboxylic acids examples include malonic, dimethylmaIonic, succinic, dodecanedioic, glutaric, adipic, trimethyladipic, pimelic, 2,2-dimethylglutaric, azelaic, sebacic,
  • 2,5-norbornanedicarboxylic diphenic, 4,4'-oxydibenzoic, diglycolic, thiodipropionic, 4,4'-sulfonyldibenzoic, 1,8-naphthalenedicarboxylic, and 2,5-naphthalene- dicarboxylic.
  • the anhydride, acid chloride, and ester derivatives of the above acids may also be used.
  • dicarboxylate ester are isophthalic acid, terephthalic acid, dimethyl terephthalate, and dimethyl isophthalate.
  • One aspect of this invention concerns the amount of 2,6- or 2,7-naphthalenediyl modification necessary for a given dicarboxylic acid or dicarboxylic acid combination to result in a polymer having a Tg above 89°C.
  • the amount of 2,6- or 2,7-naphthalenediyl modification will decrease in the order: aliphatic > cycloaliphatic > aromatic. Increasing the chain length of an aliphatic acid will result in a corresponding decrease in Tg, thus, requiring a higher level of naphthalenic modification.
  • sulfopolyester consists of a diol selected from suitable aliphatic diols, cycloaliphatic diols, aromatic diols and combinations thereof.
  • suitable aliphatic diols selected from suitable aliphatic diols, cycloaliphatic diols, aromatic diols and combinations thereof.
  • the aliphatic diols selected from suitable aliphatic diols, cycloaliphatic diols, aromatic diols and combinations thereof.
  • the diol component may also include mixtures of diols. Included within the class of aliphatic diols are
  • aliphatic diols having ether linkages such as polydiols having 4 to 800 carbon atoms.
  • Suitable diols include: ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol,
  • the diol(s) are ethylene glycol, combinations of ethylene glycol with diethylene glycol, combinations of diethylene glycol with 1,4-cyclohexane- dimethanol, combinations of ethylene glycol with
  • 1,4-cyclohexanedimethanol and combinations of ethylene glycol or diethylene glycol with a variety of suitable co-diols.
  • suitable co-diols The particular combination of diols is
  • An aspect of the present invention concerns the effect of diol chain length on the Tg of the resulting product.
  • the structures: HO-CH 2 -(CH 2 ) n -OH and HO-(OCH 2 -CH 2 ) x -OH refer to the homologous series' of diols that are composed of methylene and oxyethylene subunits. Values of n for HO-CH 2 -(CH 2 ) n -OH are normally in the range from 1 to 12. As n increases the Tg for a resulting homopolyester resin is decreased accordingly.
  • x In the case of HO-(OCH 2 -CH 2 ) x -OH, referred to as poly(ethylene glycol) or PEG, the value of x will be 10 to 50, preferably about 20, which translates into a PEG monomer molecular weight of at least 500, preferably about 1000. Typically less than 5 mole percent of PEG incorporation, based on total diol, will be used since a Tg of greater than 89°C. is required.
  • One advantage of high molecular weight PEG modification is the ability to attain higher molecular weights without losing
  • a low molecular weight determined by an inherent viscosity measurement of less than 0.1 dl/g may result in poor physical properties such as low Tg and inadequate tensile strength.
  • the difunctional sulfomonomer, component (d), of the sulfopolyester may be a dicarboxylic acid or an ester thereof containing a metal sulfonate group
  • Suitable metal cations of the sulfonate salt may be Na + , Li + , K + , Mg ++ , Ca ++ , Ni ++ , Fe ++ , Fe +++ , Zn ++ and substituted ammonium.
  • substituted ammonium refers to ammonium substituted with an alkyl or hydroxy alkyl radical having 1 to 4 carbon atoms. It is within the scope of this invention that the sulfonate salt is non-metallic and can be a nitrogenous base as described in U. S. Patent 4,304,901 which is incorporated herein by reference.
  • Monovalent alkali metal ions yield polyesters that are less readily dissipated by cold water and more readily dissipated by hot water, while divalent and trivalent metal ions result in polyesters that are not ordinarily easily dissipated by cold water but are more readily dispersed in hot water.
  • either of the different sets of properties may be desirable. It is possible to prepare the
  • sulfopolyester using, for example, a sodium sulfonate salt and later by ion-exchange replace this ion with a different ion, for example, calcium, and thus alter the characteristics of the polymer.
  • this procedure is superior to preparing the polymer with divalent salts inasmuch as the sodium salts are usually more soluble in the polymer manufacturing components than are the divalent metal salts.
  • Polymers containing divalent and trivalent metal ions are normally less elastic and rubber-like than polymers containing monovalent ions.
  • the difunctional sulfomonomer contains at least one sulfonate group attached to an aromatic nucleus wherein the functional groups are hydroxy, carboxy or amino.
  • Advantageous difunctional sulfomonomer components are those wherein the sulfonate salt group is attached to an aromatic acid nucleus such as benzene, naphthalene, diphenyl, oxydiphenyl, sulfonyldiphenyl or methylenediphenyl nucleus.
  • sulfomonomers include sulfophthalic acid, sulfoterephthalic acid, sulfoisophthalic acid, 5-sodiosulfoisophthalic acid,
  • Metallosulfoaryl sulfonate which is described in U.S. Pat. No. 3,779,993, and is incorporated herein by reference, may also be used as a sulfomonomer.
  • the sulfomonomer is present in an amount to provide water-dispersibility to the sulfopolyester. It is possible to adjust the water-dispersibility of the sulfopolyester by varying the mole percentage of
  • the sulfomonomer is present in an amount of from 5 to 40 mole percent, more
  • Semi-crystalline and amorphous materials are within the scope of the present invention. It is to be
  • the sulfopolyesters of this invention contain substantially equal molar proportions of acid equivalents (100 mole%) to hydroxy equivalents (100 mole%).
  • the sulfopolyester comprised of
  • components (a), (b), (c), and (d) will have a total of acid and hydroxyl equivalents equal to 200 mole percent.
  • the sulfopolyesters have an inherent viscosity of 0.1 to 1.0 dl/g, preferably 0.2 to 0.6 dl/g.
  • a buffer is preferably added to the compositions of the present invention. Buffers and their use are well known in the art and do not require extensive
  • Preferred buffers include sodium acetate, potassium acetate, lithium acetate, sodium phosphate monobasic, potassium phosphate dibasic and sodium carbonate.
  • the buffer is present in an amount of up to 0.2 moles per mole of difunctional sulfomonomer.
  • the buffer is present in an amount of about 0.1 moles per mole of difunctional sulfomonomer.
  • the sulfopolyesters can be prepared by conventional polycondensation procedures well-known in the art. Such processes include direct condensation of the
  • a typical procedure consists of two stages.
  • the first stage known as ester-interchange or esterification, is conducted in an inert atmosphere at a temperature of 175°C. to 240°C. for 0.5 to 8 hours, preferably 1 to 4 hours.
  • the diols depending on their particular
  • the second stage referred to as polycondensation, is conducted under reduced pressure at a temperature of 230°C. to 350°C, preferably 265°C. to 325°C, and more preferably 270°C. to 290°C. for 0.1 to 6 hours,
  • Suitable catalysts include, but are not limited to, alkoxy titanium compounds, alkali metal hydroxides and alcoholates, salts of organic carboxylic acids, alkyl tin compounds and metal oxides.
  • the sulfopolyesters of this invention are useful as adhesives, coating materials, sizes, laminated products, aqueous printing inks, and films. Particular utility is found in applications where increased abrasion
  • CARBOWAX 600 is a trademark for a polyethylene glycol having a number average molecular weight (Mn) of 600 daltons.
  • Glass transition temperature (Tg) was determined using a differential scanning calorimeter (DSC).
  • I.V. Inherent viscosity
  • a 500 mL flask was equipped with a head having a nitrogen inlet, a sidearm to allow removal of volatile materials, and a socket joint to accommodate a stirrer.
  • the stirrer shaft was inserted through the socket joint and has a ball joint attached by pressure tubing to the shaft, which provides a vacuum seal.
  • the flask is charged with 29.1 grams (0.15 moles) dimethylisophthalate, 61.0 grams (0.25 moles)
  • transesterification stage was conducted at 200°C. for two hours and 215°C. for two hours with the continuous removal of methanol by distillation.
  • the second stage also known as the polymerization stage, was performed at a reduced pressure between 0.05 to 0.5 mm Hg at a temperature of 280°C. for ten minutes.
  • Example 1 A polyester was prepared with 81 mole% isophthalic acid, 19 mole% 5-sodiosulfoisophthalate and a diol mix of 86 mole% 1,4-cyclohexanedimethanol,
  • Example 1 The apparatus and procedure used is described in Example 1.
  • a polyester was prepared with 29 mole% isophthalic acid, 52 mole% dimethyl-2,6-naphthalene- dicarboxylate, 19 mole% 5-sodiosulfoisophthalate and a diol mix of 87 mole% 1,4-cyclohexanedimethanol, 10 mole% ethylene glycol, and 3 mole% diethylene glycol.
  • Table I The test results are summarized in Table I.
  • Example 1 A polyester was prepared with 5 mole% sebacic acid, 77 mole% dimethyl-2,6-naphthalenedicarboxylate, 18 mole% 5-sodiosulfoisophthalate and a diol mix of 94 mole% ethylene glycol and 6 mole%
  • Example 1 A polyester was prepared with 13 mole% sebacic acid, 69 mole% dimethyl-2,6-naphthalene- dicarboxylate, 18 mole% 5-sodiosulfoisophthalate and a diol mix of 95 mole% ethylene glycol and 5 mole%
  • Example 2 A polyester was prepared with 2 mole% succinic acid, 79 mole% dimethyl-2,6-naphthalene- dicarboxylate, 19 mole% 5-sodiosulfoisophthalate and a diol component of ethylene glycol.
  • the test results are summarized in Table I.
  • Example 1 A polyester was prepared with 10 mole% succinic acid, 71 mole% dimethyl-2,6-naphthalene-dicarboxylate, 19 mole% 5-sodiosulfoisophthalate and a diol component of ethylene glycol.
  • the test results are summarized in Table I.
  • Examples 5 to 8 illustrate how the molar amount of incorporation and chain length of an aliphatic acid lowers the Tg of a polymer based on naphthalene units.
  • Example 1 Two polyesters containing approximately 21 mole% 5-sodiosulfoisophthalate and approximately 80 mole% 1,4-cyclohexanedimethanol are modified with 0.3 and 1.7 mole% of a polyethylene glycol having a
  • SIP level are determined to have Tg's of 98 and 100°C. for SIP levels of 15 and 20 mole%, respectively.
  • the amounts and test results are summarized in Table I.
  • Example 1 Two polyesters containing different diol. ratios of DEG/EG are compared which shows the critical nature of the diol component to Tg. The ratios and test results are summarized in Table I.
  • Examples 15-17 illustrate that both the molar amount of incorporation and chain length of an aliphatic glycol affects the Tg of a particular
  • CHDM 1,4-cyclohexanedimethanol
  • T terephthalic acid or dimethyl terephthalate
  • N dimethyl-2,6-naphthalene dicarboxylate
  • PEG600 poly(ethylene glycol)
  • PEG1000 polyethylene glycol
  • Example 18-27 a parallel plate mechanical spectrometer was used to determine the melt viscosities at 275°C. over a range of frequencies.
  • An Instron capillary rheometer was used to obtain melt viscosity data for Examples 27 and 28 at 275°C. over a range of shear rates.
  • isophthalate composition but results in a lower melt viscosity even though the level of SIP is higher for the modified system.
  • the compositional and characterization data for the polyesters used in the melt viscosity determinations are provided in Table II.
  • isophthalate/naphthalate system may have a significantly higher molecular weight and lower melt viscosity than an all-naphthalate composition without significantly lowering the Tg.
  • the compositional and characterization data for the polyesters used in the melt viscosity determinations are provided in Table II.
  • Examples 24 and 25 indicate that the modified systems have lower melt viscosities at much higher molecular weights.
  • the all-naphthalene. composition contains predominately EG while the modified composition is mainly CHDM; normally CHDM results in a higher melt viscosity than EG.
  • the compositional and characterization data for the polyesters used in the melt viscosity determinations are provided in Table II.
  • Examples 26 and 27 are comparative examples which indicate that increasing the cycloaliphatic diol (i.e., CHDM) content, while decreasing the glycol ether (i.e., DEG) content, results in a higher melt viscosity.
  • CHDM cycloaliphatic diol
  • DEG glycol ether
  • polyesters used in the melt viscosity determinations are provided in Table II.
  • Viscosity Frequency Pulascal-second (radian/second)
  • Viscosity Frequency Pulascal-second (radian/second)
  • Viscosity Frequency Pulascal-second (radian/second)
  • Viscosity Frequency Pulascal-second (radian/second)
  • polyesters based on naphthalenediyl modification have lower melt viscosities than compositions having only napthalenediyl units.
  • the compositions modified with naphthalenediyl units also have lower melt viscosities than the higher Tg water-dispersible polyesters
  • compositions containing isophthalate and naphthalenediylic units retain a high Tg, however, particular compositions having a given Tg will have lower melt viscosities than compositions possessing only naphthalenediyl units at the same given Tg.
  • compositions based on only isophthaloyl units having Tg values in the 80°C. to 89°C. range also have higher melt viscosities than the compositions containing both isophthalate and

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Polyesters Or Polycarbonates (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
PCT/US1994/007850 1993-07-23 1994-07-13 Heat-resistant water-dispersible sulfopolyester compositions Ceased WO1995003349A1 (en)

Priority Applications (4)

Application Number Priority Date Filing Date Title
JP50520195A JP3369566B2 (ja) 1993-07-23 1994-07-13 耐熱性水分散性スルホポリエステル組成物
CA002166543A CA2166543C (en) 1993-07-23 1994-07-13 Heat-resistant water-dispersible sulfopolyester compositions
EP94922540A EP0710259B1 (en) 1993-07-23 1994-07-13 Heat-resistant water-dispersible sulfopolyester compositions
DE69413694T DE69413694T2 (de) 1993-07-23 1994-07-13 Wärmebeständige wasserdispergierbare sulfopolyester zusammensetzungen

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US095,464 1993-07-23
US08/095,464 US5369210A (en) 1993-07-23 1993-07-23 Heat-resistant water-dispersible sulfopolyester compositions

Publications (1)

Publication Number Publication Date
WO1995003349A1 true WO1995003349A1 (en) 1995-02-02

Family

ID=22252150

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US1994/007850 Ceased WO1995003349A1 (en) 1993-07-23 1994-07-13 Heat-resistant water-dispersible sulfopolyester compositions

Country Status (7)

Country Link
US (1) US5369210A (enExample)
EP (1) EP0710259B1 (enExample)
JP (1) JP3369566B2 (enExample)
AT (1) ATE171714T1 (enExample)
CA (1) CA2166543C (enExample)
DE (1) DE69413694T2 (enExample)
WO (1) WO1995003349A1 (enExample)

Families Citing this family (38)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0709419B1 (en) * 1994-10-24 2004-04-14 Eastman Chemical Company Water-dispersible block copolyesters
US6384108B1 (en) 1995-09-29 2002-05-07 Xerox Corporation Waterfast ink jet inks containing an emulsifiable polymer resin
US6025412A (en) * 1995-09-29 2000-02-15 Xerox Corporation Colored particulates for ink jet inks
DK0946647T3 (da) 1996-12-19 2002-10-21 Johnson S C Comm Markets Inc Dispersioner af blandede polycarboxypolyamid-harpikser og alkali-dispergerbare harpikser samt fremstilling og anvendelse af dispersionerne
FR2760643B1 (fr) * 1997-03-14 1999-04-16 Rhodia Chimie Sa Procede de gelification de milieux aqueux, utilisation de copolyesters comme agents gelifiants de milieux aqueux et nouveaux copolyesters gelifiants de milieux aqueux
US20040024102A1 (en) * 2002-07-30 2004-02-05 Hayes Richard Allen Sulfonated aliphatic-aromatic polyetherester films, coatings, and laminates
US7625994B2 (en) 2002-07-30 2009-12-01 E.I. Du Pont De Nemours And Company Sulfonated aliphatic-aromatic copolyetheresters
US20040260034A1 (en) 2003-06-19 2004-12-23 Haile William Alston Water-dispersible fibers and fibrous articles
US7892993B2 (en) 2003-06-19 2011-02-22 Eastman Chemical Company Water-dispersible and multicomponent fibers from sulfopolyesters
US8513147B2 (en) 2003-06-19 2013-08-20 Eastman Chemical Company Nonwovens produced from multicomponent fibers
US7687143B2 (en) 2003-06-19 2010-03-30 Eastman Chemical Company Water-dispersible and multicomponent fibers from sulfopolyesters
US7635745B2 (en) 2006-01-31 2009-12-22 Eastman Chemical Company Sulfopolyester recovery
US20080167440A1 (en) * 2007-01-10 2008-07-10 Pickel Deanna L Use of copolymerizable sulfonate salts to promote char formation in polyesters and copolyesters
US9062202B2 (en) * 2007-02-26 2015-06-23 Hexion Inc. Resin-polyester blend binder compositions, method of making same and articles made therefrom
US8512519B2 (en) 2009-04-24 2013-08-20 Eastman Chemical Company Sulfopolyesters for paper strength and process
US20120183861A1 (en) 2010-10-21 2012-07-19 Eastman Chemical Company Sulfopolyester binders
US8580872B2 (en) 2011-07-21 2013-11-12 Eastman Chemical Company Sulfopolyester polymer compositions with improved water dispersibility
US8882963B2 (en) 2012-01-31 2014-11-11 Eastman Chemical Company Processes to produce short cut microfibers
JP6036004B2 (ja) * 2012-08-22 2016-11-30 東洋紡株式会社 ポリエステル樹脂
US9303357B2 (en) 2013-04-19 2016-04-05 Eastman Chemical Company Paper and nonwoven articles comprising synthetic microfiber binders
US9598802B2 (en) 2013-12-17 2017-03-21 Eastman Chemical Company Ultrafiltration process for producing a sulfopolyester concentrate
US9605126B2 (en) 2013-12-17 2017-03-28 Eastman Chemical Company Ultrafiltration process for the recovery of concentrated sulfopolyester dispersion
US9650539B2 (en) 2014-10-27 2017-05-16 Eastman Chemical Company Thermosetting compositions based on unsaturated polyesters and phenolic resins
US9487619B2 (en) 2014-10-27 2016-11-08 Eastman Chemical Company Carboxyl functional curable polyesters containing tetra-alkyl cyclobutanediol
US9598602B2 (en) 2014-11-13 2017-03-21 Eastman Chemical Company Thermosetting compositions based on phenolic resins and curable poleyester resins made with diketene or beta-ketoacetate containing compounds
US20160340471A1 (en) 2015-05-19 2016-11-24 Eastman Chemical Company Aliphatic polyester coating compositions containing tetramethyl cyclobutanediol
US12624161B2 (en) 2015-06-19 2026-05-12 Stratasys, Inc. Water dispersible polymer for use in additive manufacturing
CN107810215B (zh) 2015-06-19 2020-08-07 斯特塔思有限公司 用于增材制造的水分散性聚合物
US20170088665A1 (en) 2015-09-25 2017-03-30 Eastman Chemical Company POLYMERS CONTAINING CYCLOBUTANEDIOL AND 2,2 BIS(HYDROXYMETHYL) AlKYLCARBOXYLIC ACID
US9988553B2 (en) 2016-02-22 2018-06-05 Eastman Chemical Company Thermosetting coating compositions
US10011737B2 (en) 2016-03-23 2018-07-03 Eastman Chemical Company Curable polyester polyols and their use in thermosetting soft feel coating formulations
WO2019075107A1 (en) 2017-10-10 2019-04-18 Stratasys, Inc. WATER-DISPERSIBLE THERMOPLASTIC MATERIAL COMPRISING A SULFINATED COPOLYMER FOR USE IN ADDITIVE MANUFACTURE
EP3864093B1 (en) 2018-10-10 2026-08-05 Stratasys, Inc. Water dispersible sulfonated thermoplastic copolymer for use in additive manufacturing
WO2020201921A1 (en) * 2019-03-29 2020-10-08 3M Innovative Properties Company Composition and article comprising the same
WO2022010963A1 (en) * 2020-07-08 2022-01-13 Bostik, Inc. Amorphous copolyester resin for industrial coatings and methods for coating a metal surface using such coating compositions
US20230312818A1 (en) * 2020-08-07 2023-10-05 Eastman Chemical Company Sulfopolyesters comprising diethylene glycol and ethylene gylcol
US12157800B2 (en) * 2021-04-12 2024-12-03 Stratasys, Inc. Method for underwater processing of water-dispersible materials
WO2023111593A1 (en) 2021-12-17 2023-06-22 Sun Chemical Corporation Thermally resistant aqueous inks

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS5740525A (en) * 1980-08-22 1982-03-06 Toyobo Co Ltd Aqueous dispersion
WO1992013021A1 (en) * 1991-01-25 1992-08-06 Eastman Kodak Company Modified polyester useful as photographic roll film support
JPH04332756A (ja) * 1991-05-09 1992-11-19 Teijin Ltd ポリエステル水分散体及びこれを塗布した易接着性ポリエステルフイルム
JPH0586174A (ja) * 1991-09-30 1993-04-06 Toray Ind Inc 共重合ポリエステル

Family Cites Families (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US3123587A (en) * 1964-03-03 Polyester wash-wear fabric
US3018272A (en) * 1955-06-30 1962-01-23 Du Pont Sulfonate containing polyesters dyeable with basic dyes
US3436376A (en) * 1967-05-19 1969-04-01 Sun Oil Co Polyesters
US3563942A (en) * 1967-11-29 1971-02-16 Du Pont Aqueous dispersion of copolyesters modified with a sulfonated aromatic compound
US3546008A (en) * 1968-01-03 1970-12-08 Eastman Kodak Co Sizing compositions and fibrous articles sized therewith
US3779993A (en) * 1970-02-27 1973-12-18 Eastman Kodak Co Polyesters and polyesteramides containing ether groups and sulfonate groups in the form of a metallic salt
US3734874A (en) * 1970-02-27 1973-05-22 Eastman Kodak Co Polyesters and polyesteramides containing ether groups and sulfonate groups in the form of a metallic salt
US4480085A (en) * 1983-09-30 1984-10-30 Minnesota Mining And Manufacturing Company Amorphous sulfopolyesters

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS5740525A (en) * 1980-08-22 1982-03-06 Toyobo Co Ltd Aqueous dispersion
WO1992013021A1 (en) * 1991-01-25 1992-08-06 Eastman Kodak Company Modified polyester useful as photographic roll film support
JPH04332756A (ja) * 1991-05-09 1992-11-19 Teijin Ltd ポリエステル水分散体及びこれを塗布した易接着性ポリエステルフイルム
JPH0586174A (ja) * 1991-09-30 1993-04-06 Toray Ind Inc 共重合ポリエステル

Non-Patent Citations (3)

* Cited by examiner, † Cited by third party
Title
DATABASE WPI Week 8215, Derwent World Patents Index; AN 82-29901E *
DATABASE WPI Week 9301, Derwent World Patents Index; AN 93-004695 *
DATABASE WPI Week 9318, Derwent World Patents Index; AN 93-149282 *

Also Published As

Publication number Publication date
JP3369566B2 (ja) 2003-01-20
DE69413694T2 (de) 1999-02-25
DE69413694D1 (de) 1998-11-05
EP0710259A1 (en) 1996-05-08
CA2166543A1 (en) 1995-02-02
US5369210A (en) 1994-11-29
JPH09500677A (ja) 1997-01-21
ATE171714T1 (de) 1998-10-15
EP0710259B1 (en) 1998-09-30
CA2166543C (en) 2000-10-31

Similar Documents

Publication Publication Date Title
US5369210A (en) Heat-resistant water-dispersible sulfopolyester compositions
US5369211A (en) Water-dispersible sulfo-polyester compostions having a TG of greater than 89°C.
EP1159329B1 (en) Water-dispersible polyesters
US5571620A (en) Water-dispersible copolyester-ether compositions
US5709940A (en) Water-dispersible block copolyesters
US5017679A (en) Polyesters terminated with carboxycyclohexanecarboxylate groups
EP1103578B1 (en) Water-dispersible films and fibers based on sulfopolyesters
US4390687A (en) High melt strength elastometric copolyesters
US4396746A (en) Thermoplastic polyester copolymer
KR20160014029A (ko) 1 초과의 전하 밀도를 갖는 설포폴리에스터 및 이로부터 제조된 제품
EP1135426A1 (en) Terephthalate-based sulfopolyesters
US5698626A (en) Functional group terminated polymers containing sulfonate group via polymerization of sulfonated monomers
EP0075527B1 (en) High melt strength elastomeric copolyesters
US5342902A (en) Poly(ester-ether) compositions having increased thermal stability
WO2003050160A1 (en) Antistatic polyester-polyethylene glycol compositions
JPH04285631A (ja) 熱可塑性ポリエステルエラストマー
JP2665074B2 (ja) ポリエステルの製造方法
WO2003022907A1 (en) Copolyether composition and processes therefor and therewith
JPH04279631A (ja) 共重合ポリエステル

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): CA JP

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE

DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
121 Ep: the epo has been informed by wipo that ep was designated in this application
WWE Wipo information: entry into national phase

Ref document number: 2166543

Country of ref document: CA

WWE Wipo information: entry into national phase

Ref document number: 1994922540

Country of ref document: EP

WWP Wipo information: published in national office

Ref document number: 1994922540

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 1994922540

Country of ref document: EP