KR890002433A - 내식 내마모성이 우수한 Fe기 육성합금 - Google Patents

내식 내마모성이 우수한 Fe기 육성합금 Download PDF

Info

Publication number
KR890002433A
KR890002433A KR1019880007460A KR880007460A KR890002433A KR 890002433 A KR890002433 A KR 890002433A KR 1019880007460 A KR1019880007460 A KR 1019880007460A KR 880007460 A KR880007460 A KR 880007460A KR 890002433 A KR890002433 A KR 890002433A
Authority
KR
South Korea
Prior art keywords
excellent corrosion
resistance
corrosion resistance
based growth
growth alloy
Prior art date
Application number
KR1019880007460A
Other languages
English (en)
Other versions
KR910003575B1 (ko
Inventor
나데에이 야브기
사브로우 와기다
Original Assignee
나가노 다께시
미쯔비시 긴조구 가부시기가이샤
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 나가노 다께시, 미쯔비시 긴조구 가부시기가이샤 filed Critical 나가노 다께시
Publication of KR890002433A publication Critical patent/KR890002433A/ko
Application granted granted Critical
Publication of KR910003575B1 publication Critical patent/KR910003575B1/ko

Abstract

내용 없음

Description

내식 내마모성이 우수한 Fe기 육성합금
본 내용은 요부공개 건이므로 전문내용을 수록하지 않았음

Claims (4)

  1. C 0.005 - 1.6%
    Mn 4 - 28%
    Cr 12 - 36%
    Mo 0.01 - 9%
    Hf 0.005 - 15%
    N 0.01 - 0.9%
    를 함유하고 나머지 Fe와 불가피 불순물로 되는 조성(이상 중량%)을 가짐을 특징으로 한 내식 내마모성이 우수한 Fe기 육성합금.
  2. C 0.005 - 1.6%
    Mn 4 - 28%
    Cr 12 - 36%
    Mo 0.01 - 9%
    Hf 0.005 - 15%
    N 0.01 - 0.9%
    Si 0.01 - 5%
    Ni 5 - 30%
    를 함유하고 나머지 Fe와 불가피 불순물로 되는 조성(이상 중량%)을 가짐을 특징으로 한 내식 내마모성이 우수한 Fe기 육성합금.
  3. C 0.005 - 1.6%
    Mn 4 - 28%
    Cr 12 - 36%
    Mo 0.01 - 9%
    Hf 0.005 - 15%
    N 0.01 - 0.9%를 함유하고 그리고
    Nb 0.01 - 6%
    W 0.01 - 6% 중의 1종 또는 2종을 함유하며 나머지 Fe와 불가피 불순물로 되는 조성(이상 중량%)을 가짐을 특징으로 한 내식 내마모성이 우수한 Fe기 육성합금.
  4. C 0.005 - 1.6%
    Mn 4 - 28%
    Cr 12 - 36%
    Mo 0.01 - 9%
    Hf 0.005 - 15%
    N 0.01 - 0.9%
    Si 0.01 - 5%
    Ni 5 - 30%
    를 함유하고 그리고 Nb 0.01 - 6%, W 0.01 - 6%중의 일종 또는 2종을 하뮤하고 나머지 Fe와 불가피 불순물로 되는 조성(이상 중량%)을 가짐을 특징으로 한 내식 내마모성이 우수한 Fe기 육성합금.
    ※참고사항 : 최초출원 내용에 의하여 공개하는 것임.
KR1019880007460A 1987-07-16 1988-06-21 내식 내마모성이 우수한 Fe기 육성합금 KR910003575B1 (ko)