JPH1025554A - インバータ制御コンプレッサーモーター用の無方向性電磁鋼板 - Google Patents

インバータ制御コンプレッサーモーター用の無方向性電磁鋼板

Info

Publication number
JPH1025554A
JPH1025554A JP8181007A JP18100796A JPH1025554A JP H1025554 A JPH1025554 A JP H1025554A JP 8181007 A JP8181007 A JP 8181007A JP 18100796 A JP18100796 A JP 18100796A JP H1025554 A JPH1025554 A JP H1025554A
Authority
JP
Japan
Prior art keywords
case
motor
regulated
steel sheet
efficiency
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP8181007A
Other languages
English (en)
Other versions
JP3527020B2 (ja
Inventor
Takahide Shimazu
高英 島津
Masaki Harada
正軌 原田
Kuniyasu Ikeda
邦泰 池田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Corp
Original Assignee
Nippon Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Steel Corp filed Critical Nippon Steel Corp
Priority to JP18100796A priority Critical patent/JP3527020B2/ja
Publication of JPH1025554A publication Critical patent/JPH1025554A/ja
Application granted granted Critical
Publication of JP3527020B2 publication Critical patent/JP3527020B2/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

(57)【要約】 【課題】 本発明は、高効率なインバータ制御コンプレ
ッサーモーター用の無方向性電磁鋼板を提供する。 【解決手段】 板厚が0.3〜0.6mmであって、表面
粗度Raが0.6μm以下、固有抵抗が40〜75μΩ
・cm、かつ最終歪取り焼鈍後の結晶粒径が40〜12
0μmであることを特徴とするインバータ制御コンプレ
ッサーモーター用の無方向性電磁鋼板。

Description

【発明の詳細な説明】
【0001】
【発明の属する技術分野】本発明は、冷暖房用エアコン
または冷蔵庫などインバータ制御コンプレッサーモータ
ーに使用するとモーター効率が従来より大幅に向上する
無方向性電磁鋼板に関するものである。
【0002】
【従来の技術】近年、石油価格の高騰によるエネルギー
消費低減要請から、モーターの電気消費量の改善が求め
られている。特に、連続運転されることの多い冷蔵庫や
エアコン用モーターに高効率化要求が強い。このため、
この分野ではモーター効率改善を目的として、従来のO
N−OFF制御から、連続でモーターの回転数を周波数
で自動制御するインバータ駆動方式に変更されてきてい
る。しかしながら、更なる効率を求めて競争は激しく、
電気制御機構の改善だけでは限界にきている。冷蔵庫や
エアコン用モーターは、ガスを循環させるコンプレッサ
ーモーターとも称される。周知のごとく、モーター用鋼
板には無方向性電磁鋼板が使用される。
【0003】無方向性電磁鋼板は、通常Si:4%以
下、Al:2%以下を含有して、厚みが0.2〜0.7
mmの鋼板である。無方向性電磁鋼板の製造方法として
は、幾つか知られているが、主なものとしては最終焼鈍
をするものと最終スキンパス圧延をするものとがある。
【0004】従来、コンプレッサーモーター用にはセミ
プロセス無方向性電磁鋼板が用いられることが多かっ
た。すなわち、モーターコアへ打抜いた後、打抜きの歪
み除去と結晶粒成長を兼ねて鉄損を改善するための歪取
り焼鈍が必須だからである。このため、歪取り焼鈍を前
提として、スキンパスによる歪み誘起粒成長を利用した
製鉄メーカーでの最終スキンパス圧延を施した所謂、ス
キンパス材が用いられることが多かった。
【0005】スキンパス材は、歪取り焼鈍によって結晶
粒径がほぼ150μm程度に粒成長する。また、鉄損対
策としての磁束密度を重視する立場から、磁気スピンを
持たないSi,Alなどの量が比較的少ない無方向性電
磁鋼板が利用されていた。しかしながら、これら従来の
無方向性電磁鋼板では、さらなるモーター効率の改善に
はつながらなかった。
【0006】
【発明が解決しようとする課題】本発明は上記の点に鑑
み、冷暖房用エアコンまたは冷蔵庫などのモーターに使
用される高効率のインバーター制御コンプレッサーモー
ター用の無方向性電磁鋼板を提供する。
【0007】
【課題を解決するための手段】本発明は、板厚が0.3
〜0.6mmであって、表面粗度Raが0.6μm以下、
固有抵抗が40〜75μΩ・cm、かつ最終歪取り焼鈍
後の結晶粒径が40〜120μmであることを特徴とす
るインバータ制御コンプレッサーモーター用の無方向性
電磁鋼板である。
【0008】本発明のポイントは2点ある。1点目はイ
ンバータ制御をする場合のコンプレッサーモーターの効
率を改善するためには、無方向性電磁鋼板の板厚、表面
粗度、固有抵抗、結晶粒径を制御すればよいこと。2点
目は、板厚、表面粗度、固有抵抗、結晶粒径を特定範囲
に規制することは、工業的に十分可能なことである。
【0009】
【発明の実施の形態】以下、本発明の限定理由について
説明する。板厚は、0.3mm以上かつ0.6mm以下とす
る。0.3mm未満では板厚が薄すぎて鋼板の剛性が足り
なくモーターコアのティース部での曲がり・折れなどが
生じやすく、0.6mmを超えると鉄損が大きくなるため
である。
【0010】表面粗度Raは、0.6μm以下に制限す
る。表面粗度Raが0.6μmを超えると打抜き後にコ
アを積層した時の占積率の低下が大きくなり、有効な断
面積当たりの磁束密度が低下し、モーター効率が劣化す
るためである。なお、ここで表面粗度Raとは、中心線
平均粗さをいうものとする。
【0011】固有抵抗は、40μΩ・cm以上かつ75
μΩ・cm以下とする。40μΩ・cm未満ではインバ
ーター制御用のモーターとしては効率不足なためであ
る。固有抵抗を上げるためには、例えばBozorth “ FER
ROMAGNETISM ”,40P ,1951に記載のようにSi,A
l,Mn,Cu,Mo,Ni,W,Coなどを添加すれ
ばよいが、75μΩ・cmを超える固有抵抗を得るため
にはSi+Al%で5%以上必要なため、脆性の問題か
ら工業的な生産が難しく磁束密度が劣化してモーター効
率が低下するため避ける。
【0012】歪取り焼鈍後の結晶粒径は、40μm以上
かつ120μm以下とする。40μm未満の細粒では磁
束密度が悪く目的の磁気特性が得られない。また、12
0μmを超えると高周波の鉄損が劣化してインバータ駆
動のモーター効率が確保できない。なお、ここで結晶粒
径とは、板厚断面方向の平均結晶粒径をいうものとす
る。
【0013】以上のように板厚、表面粗度、固有抵抗、
結晶粒径を制御することが、インバータ制御コンプレッ
サーモーター用の素材には必要である。モーター効率と
磁気特性の関係については従来より不明確な部分が多
く、エプスタインでの鉄損測定値の10〜40倍ものエ
ネルギー損失が実際のモーターで発生しており、鉄損と
磁束密度だけでは整理できなかった。モーター効率に影
響を与える要因として、無方向性電磁鋼板の素材の特性
である鉄損と磁束密度以外に、モーター設計に関わるエ
アーギャップや機械損失などが知られており、項目が多
くて複雑である。更に、磁気特性について述べれば、実
機のモーターコアでは磁束の回転あるいはコアの部位に
よって磁束密度が異なることを考慮しなければならな
い。周波数に関しても、インバータ制御の入力電流波形
は歪が大きく、また基本周波数に高周波を重畳したもの
が多くて非常に複雑である。つまり、従来の周波数が5
0または60Hzに固定された波形に比べて、高周波成分
が多くなっているのが特徴である。このため、従来のモ
ーターコアと比較して特に、高周波によるうず電流が増
加し、うず電流を減少させるための固有抵抗、板厚や結
晶粒径の効果が大きく出たものと考えられる。
【0014】本発明鋼の具体的な製造方法の一例を示す
と以下の通りである。重量%でC:0.002%、S
i:2.5%、Al:0.2%、Mn:0.35%、
P:0.02%、S:0.001%、N:0.001%
を含む連続鋳造スラブを1000℃に加熱して、仕上温
度900℃、巻取り温度600℃で2mmの熱延コイルを
製造した。これを1000℃で連続焼鈍後、酸洗、表面
粗度Raが0.25μmのロールを用いて冷延して0.
5mm厚とした。次いで、脱脂後、900℃で連続焼鈍
し、絶縁被膜を塗布焼き付けした。得られた鋼板の特性
値は、板厚が0.5mm、表面粗度が0.18μmRa、
固有抵抗が43μΩ・cm、結晶粒径が60μmであ
り、本発明鋼の条件を満たすものであった。
【0015】なお、結晶粒径については、最終焼鈍での
温度×時間で制御するのが簡便である。顧客での歪取り
焼鈍を実施することも可能であるが、歪取り焼鈍温度は
750℃程度なので、この鋼板では殆ど結晶粒径は変化
しなかった。また、最終スキンパス圧延を実施する場合
には、特に結晶粒径に注意しなければならない。歪取り
焼鈍で爆発的に粒成長するためである。このときは、ス
キンパス圧延での冷延率を従来の2〜7%程度より8〜
30%程度の強めの圧下にしたほうが本発明の結晶粒径
に制御しやすい。
【0016】
【実施例】成分Si,Alと伸びとが表1である無方向
性電磁鋼板を準備した。実験No.19と20は最終ス
キンパス圧延し、その他の実験No.1〜18のものは
最終連続焼鈍処理をした。鋼板表面には公知の半有機・
半無機系電気絶縁皮膜がある。固有抵抗は、ダブルブリ
ッジ法で表面被膜を除去して測定した。外径80mmのロ
ーター、外径120mmのステーターに打抜いてから10
0枚積みのコアにカシメた。このコアに750℃で2時
間歪取り焼鈍を実施し、結晶粒径を測定した。表1の磁
気特性は、エプスタイン試料での圧延方向とそれに垂直
な方向試料の平均であり、歪取り焼鈍750℃×2時間
後の値である。これをインバーター制御コンプレッサー
モーターに試作して、60回転/分でモーター効率をチ
ェックした。モーター効率は、入力電気エネルギーに対
する出力エネルギーの比をとった。入力は電圧と電流
で、出力は発電機をつなぐ方式で測定した。
【0017】
【表1】
【0018】実施例に示すように、板厚、表面粗度、固
有抵抗、結晶粒径を本発明の範囲に制御したものでは、
優れたモーター効率が得られた。また、他の回転数でも
効率のチェックをしたが、同様の結果であった。
【0019】
【発明の効果】本発明によれば、高効率なインバータ制
御コンプレッサーモーター用の無方向性電磁鋼板が得ら
れた。

Claims (1)

    【特許請求の範囲】
  1. 【請求項1】 板厚が0.3〜0.6mmであって、表面
    粗度Raが0.6μm以下、固有抵抗が40〜75μΩ
    ・cm、かつ最終歪取り焼鈍後の結晶粒径が40〜12
    0μmであることを特徴とするインバータ制御コンプレ
    ッサーモーター用の無方向性電磁鋼板。
JP18100796A 1996-07-10 1996-07-10 インバータ制御コンプレッサーモーター用の無方向性電磁鋼板 Expired - Lifetime JP3527020B2 (ja)