CN108842271A - A kind of processing method of three line of high-elastic weft-knitting liner tissue - Google Patents
A kind of processing method of three line of high-elastic weft-knitting liner tissue Download PDFInfo
- Publication number
- CN108842271A CN108842271A CN201810648538.1A CN201810648538A CN108842271A CN 108842271 A CN108842271 A CN 108842271A CN 201810648538 A CN201810648538 A CN 201810648538A CN 108842271 A CN108842271 A CN 108842271A
- Authority
- CN
- China
- Prior art keywords
- cloth
- cotton
- fabric
- dibit
- technique
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of processing methods of high-elastic three line of weft-knitting liner tissue, the yarn of plain weave is made of the high-elastic spandex of 140D, traditional weave of conventional plain weave cotton ammonification synthetic fibre has been overturned completely, also prevented it is conventional cross bottom common fault with the anti-silk of low elastic polyester filament, neat beltloop weaving technology is selected at cloth bottom;Base technique is determined in reference, greatly reduces the cloth cover wrinkle problem of heavily fabric.Dyeing and finishing of other dyeing and finishing technologies with common cotton dibit clothing cloth;The effect of spandex fabric, tensile-elasticity are 2 times of common cotton dibit clothing cloth;Cloth cover bamboo joint meteor shower, the neat effect of cloth bottom looped pile, greatly improves, and Quick-return through Weftwise stretch, is one of best improvement of common cotton dibit clothing cloth, substantially increases the class of knitted sport leisure fabric;The primary completely new revolution of common cotton dibit clothing cloth, has succession to have innovation.
Description
Technical field
The invention belongs to textile dyeing and finishing technical field, in particular to a kind of processing of three line of high-elastic weft-knitting liner tissue
Method.
Background technique
Liner tissue is divided into two kinds:Two lines pad tissue and three lines pad tissue.Two lines pad tissue, are also known as unit
Clothing, ground tissue is plain stitch, forms a complete row by two system for weaving:First system for weaving textile washer yarn
That is beltloop, second system for weaving weave wire gauze, that is, plain weave, behind woven by this circulation.Three lines pad tissue, also known as double
Position clothing is not double yarn unit clothing, their structure is completely different.Its ground tissue is plating structure, is by three braidings
System forms a complete row:First system for weaving textile washer yarn, that is, looped pile or beltloop, in weaving process, it is not needed
Kinking lopping but hung in the form of tuck on cloth bottom, so the available thicker yarn count of this group of yarn;Second system for weaving is compiled
It knits the veil in plating structure and ties up hair, referred to as " binder yarn ", it is that beltloop and plain weave connect together, and " binder yarn " is also
One total eclipse tissue, third system for weaving weave filling, that is, plain weave in plating structure, are the tissues of a total eclipse, it is formed
The basis of body;Tie up hair and " plain weave " is to move back circle simultaneously, so on cloth cover, visible two yarns of each coil
's.It is woven below by this circulation.
Dibit clothing is divided into little fish scale, fish scale and left and right tiltedly, this is to contain pin position difference by the tuck of beltloop and generate
Variation, but its weaving process be not respectively.General popular dibit clothing machine only has 16G, 18G, 20G, 22G, 24G five
Kind, the weaving of 28G is also very immature, therefore the collocation of the yarn count of dibit clothing cloth is less.There is larger leakage silk again in centre folder low stretch yarn
Risk, thus limit the variation and collocation of its yarn count.This fabric now developed has that good hand feeling, body are strong, thick and solid,
Elasticity, hygroscopicity, warmth retention property are good, and loop construction is stablized, and have good wearability, mainly make gym suit, lapel T sympathizes
The fabrics such as shirt, pyjamas, children's garment are the good selections of autumn and winter knitted sport easy suit, so have broad application prospects again.
The finished fabric tensile elasticity response rate of general dibit clothing cloth is formed, line 50% or so because tWeft Knitted Fabrics are covered by coil string
Gap is larger between circle and coil, when fabric laterally or longitudinally stretches, formed weft-knitted product coil loop pillar and circle it is dry between can
Mutually to convert, make fabric that there is good elasticity and extensibility, spandex high stretch yarn is added on conventional dual bit clothing to be made
Elasticity and extensibility more preferably, but the bigger performance space of the structural constraint of dibit clothing elasticity.How the structure of cloth had both been kept
Particularity, and the finished fabric elastic recovery energy of dibit clothing cloth is broken through, reach high resiliency, and accomplish high simultaneously through broadwise
Bullet is at the original intention studied.
Summary of the invention
The present invention overcomes the disadvantages of the prior art, provides a kind of processing of three line of high-elastic weft-knitting liner tissue
Method.The present invention is achieved by the following technical programs:
A kind of processing method of three line of high-elastic weft-knitting liner tissue, processing method include the following steps:
Step A:Raw material interweaves, direct looming weaving(Raw material is not required to do any processing);
Step B:Fabric is singed;Its technique is as follows:8 casees vertical letter door width formula framing shaping machines, 200 DEG C of temperature, machine speed 28Y/Min;
Fabric specification:The side 148cm X591G/M2;
Step C:Pre-setting;Its technique is as follows:Machine speed and cropping revolution are set:Machine speed:23 revs/min;Cropping revolution:2500
Turn/25KG;
Step D:Dyeing;
Step E:Scouring of wool and drying;Its technique is as follows:8 casees vertical letter 140 DEG C of * 28Y of door width formula framing shaping machine;
Step F:Finished product sizing;Its technique is as follows:8 casees vertical letter 170 DEG C of * 24Y of door width formula framing shaping machine:Main color fastness:It washes
Water:4 grades;Discoloration:3.5 grades or more;Staining:3.5 grades or more;It shrinks and requires:W-2%, L-2%;Twist requirement:N+0.5%, at
Product specification:The practical x430g/m2 of 168CM.
Further, the technique dyed in the step D is specially that low temperature dyeing food hair one is bathed:Time-consuming 224 ', it is neutral
Eat hair agent 0.15%;Dye formulation:Dragon contains 3RS150% 0.25%;Dragon contains 3BSN150% 0.32%;Dragon contains G 300% 5.0%;
NACL 90G/L;NA2CO3 20G/L.
Further, the raw material group becomes 32S/1 combing CVC95/5 meteor shower section coloured silk ring;32S/1 essence cotton;
140D tries to stop people from fighting each other;32S/2 cotton (strand).
As a kind of optimal technical scheme, the present invention is mainly carried out from yarn texture, dyeing flow, dyeing several respects
It improves, obtains dyeing total solution.The present invention has the characteristics that compared with prior art and beneficial effect:1. using 140D
High-elastic spandex makees the yarn of plain weave, has overturned traditional weave of conventional plain weave cotton ammonification synthetic fibre completely, has also prevented conventional use
The anti-silk of low elastic polyester filament crosses bottom common fault, and neat beltloop weaving technology is selected at cloth bottom;2. base technique is determined in reference, greatly reduce thick and heavy knit
The cloth cover wrinkle problem of object.Dyeing and finishing of other dyeing and finishing technologies with common cotton dibit clothing cloth;3. the effect of spandex fabric, tensile-elasticity
It is 2 times of common cotton dibit clothing cloth;4. cloth cover bamboo joint meteor shower, the neat effect of cloth bottom looped pile, greatly improve through Weftwise stretch,
And Quick-return, it is one of best improvement of common cotton dibit clothing cloth, substantially increases the class of knitted sport leisure fabric;
5. the primary completely new revolution of common cotton dibit clothing cloth, has succession to have innovation.
Detailed description of the invention
Present invention will be further explained below with reference to the attached drawings and examples.
Fig. 1 is the dyeing heating curve of the embodiment of the present invention 1.
Specific embodiment
Below with reference to embodiment, specific embodiments of the present invention will be described in further detail.
Embodiment 1
A kind of processing method of three line of high-elastic weft-knitting liner tissue, raw material is 32S/1 combing CVC95/5 meteor shower Duan Caizhu
Section;32S/1 essence cotton;140D tries to stop people from fighting each other;32S/2 cotton (strand), includes the following steps:Raw material looming weaving, fabric are singed, are made a reservation for
Type, dyeing, scouring of wool and drying, finished product sizing.
Step A:Raw material interweaves, direct looming weaving;(Raw material is not required to do any processing)
Weaving process:9F twill dibit clothing(FLEECE,TERRY), 9F. FLEECE(Three lines pad tissue)
Arrange needle:BCD, practical operation:Use yarn count:(32S/1 combing CVC95/5 meteor shower section coloured silk ring+32S/1 essence cotton)+
140D tries to stop people from fighting each other+32S/2 cotton (strand), board needle cun number:24G30 " 2256N single circular weft machine, knitting needle arrangement:123 knitting needle types
Number:141.52G005 G006, G007;Blade profile number:2.9MM;Water chestnut arrangement:
∧/3 group ∩ ∧ ∧-∧ ∧-∧ ∧ ,-∧ ∧ ∩ ∧ ∧-∧ ∧ ,-∧ ∧-∧ ∧ ∩ ∧, row's yarn sequence:1.
Arrange yarn in 4.7 tunnels:32S/2 cotton yarn;Arrange yarn in 2 tunnels:Yarn is arranged on 32S/1 meteor shower CVC, 5.8 tunnels:32S/1 essence cotton;3.6. yarn is arranged on 9 tunnels:
140D/1 spandex;Yarn 100 needles of long setting:Tie up hair:38CM(32S/1);Plain weave:12CM(140D/1);Beltloop:16CM(32S/2).
Raw material purposes:32S/1 combing CVC95/5 meteor shower section coloured silk ring:It increases varieties and designs and special appearance style,
5% staple fiber of washing is added, increases bony and moisture absorption sweat discharging functions;The spinning of determining of raw material also increases some imitate to a certain extent
The difficulty emitted;32S/1 essence cotton:For diluting the effect of meteor shower section coloured silk ring, it is unlikely to too fancy;140D tries to stop people from fighting each other:It does high-elastic
And want the primary raw material of spandex fabric;32S/2 cotton (strand):Accomplish the neat primary raw material of beltloop.
Weave processing method and technical requirements:The big position clothing cloth weave of single knitting machine 9F twill.It entrys mouth requirement:1.4.7
Arrange yarn in road:32S/2 cotton (stock yarn)(Dedicated yarn mouth, special neat beltloop cam design);Tie up hair row's yarn in 2 tunnels:32S/1 meteor shower
CVC;Tie up hair row's yarn in 5.8 tunnels:32S/1 essence cotton;3.6. yarn is arranged on 9 tunnels:140D/1 spandex.
Step B:Fabric is singed;Its technique is as follows:8 casees vertical letter door width formula framing shaping machines, 200 DEG C of temperature, machine speed 28Y/
Min;Fabric specification:The side 148cm X591G/M2.
Step C:Pre-setting;Its technique is as follows:Machine speed and cropping revolution are set:Machine speed:23 revs/min;Cropping revolution:
2500 turns/25KG;High-elastic latitude dibit clothing is a kind of innovation research and development product, because its performance and existing product in the market have certain difference
Not, completely new weaving operation method is needed to be applicable in it.
Step D:Dyeing;Low temperature dyeing is eaten hair one and is bathed:Time-consuming 224 ', neutrality food hair agent 0.15%;Dye formulation:Long Sheng
3RS150% 0.25%;Dragon contains 3BSN150% 0.32%;Dragon contains G 300% 5.0%;NACL 90G/L;NA2CO3 20G/L, dye
Color heating curve:60℃*90min.
Step E:Scouring of wool and drying;Its technique is as follows:8 casees vertical letter 140 DEG C of * 28Y of door width formula framing shaping machine;
Step F:Finished product sizing;Its technique is as follows:8 casees vertical letter 170 DEG C of * 24Y of door width formula framing shaping machine:Main color fastness:It washes
Water:4 grades;Discoloration:3.5 grades or more;Staining:3.5 grades or more;It shrinks and requires:W-2%, L-2%;Twist requirement:N+0.5%, at
Product specification:The practical x430g/m2 of 168CM.Influence of the heat setting process to fabric property is very big after dyeing, temperature when sizing
Degree, speed, time, pulling force must be controlled, and the characteristics such as elasticity, the feel of fabric otherwise can be destroyed.Setting temperature is no more than 170
Degree;Setting time is no more than 1 minute;Sizing breadth meet cloth cover it is smooth after cannot deliberately widen, as far as possible keep dyeing after just
Normal breadth, breadth of being otherwise formed are widened, and fabric elasticity performance is poorer.
Dye heating curve such as Fig. 1.
It is any ripe although the present invention is disclosed as above with embodiment, its protection scope being not intended to limit the invention
The technical staff for knowing this technology changes and retouches made without departing from the spirit and scope of the invention, should belong to this
The protection scope of invention.
Claims (3)
1. a kind of processing method of three line of high-elastic weft-knitting liner tissue, it is characterised in that:Its processing method includes following step
Suddenly:
Step A:Raw material interweaves, direct looming weaving;
Step B:Fabric is singed;Its technique is as follows:8 casees vertical letter door width formula framing shaping machines, 200 DEG C of temperature, machine speed 28Y/Min;
Fabric specification:The side 148cm X591G/M2;
Step C:Pre-setting;Its technique is as follows:Machine speed and cropping revolution are set:Machine speed:23 revs/min;Cropping revolution:2500
Turn/25KG;
Step D:Dyeing;
Step E:Scouring of wool and drying;Its technique is as follows:8 casees vertical letter 140 DEG C of * 28Y of door width formula framing shaping machine;
Step F:Finished product sizing;Its technique is as follows:8 casees vertical letter 170 DEG C of * 24Y of door width formula framing shaping machine:Main color fastness:It washes
Water:4 grades;Discoloration:3.5 grades or more;Staining:3.5 grades or more;It shrinks and requires:W-2%, L-2%;Twist requirement:N+0.5%, at
Product specification:The practical x430g/m2 of 168CM.
2. the processing method of three line of high-elastic weft-knitting liner tissue according to claim 1, it is characterised in that:The step
The technique dyed in rapid D is specially that low temperature dyeing food hair one is bathed:Time-consuming 224 ', neutrality food hair agent 0.15%;Dye formulation:Long Sheng
3RS150% 0.25%;Dragon contains 3BSN150% 0.32%;Dragon contains G 300% 5.0%;NACL 90G/L;NA2CO3 20G/L.
3. the processing method of three line of high-elastic weft-knitting liner tissue according to claim 1, it is characterised in that:The original
Material group becomes 32S/1 combing CVC95/5 meteor shower section coloured silk ring;32S/1 essence cotton;140D tries to stop people from fighting each other;32S/2 cotton (strand).