CN105274879A - Interweaved fabric with dreamlike color-change function and preparation technology of interweaved fabric - Google Patents
Interweaved fabric with dreamlike color-change function and preparation technology of interweaved fabric Download PDFInfo
- Publication number
- CN105274879A CN105274879A CN201510871901.2A CN201510871901A CN105274879A CN 105274879 A CN105274879 A CN 105274879A CN 201510871901 A CN201510871901 A CN 201510871901A CN 105274879 A CN105274879 A CN 105274879A
- Authority
- CN
- China
- Prior art keywords
- cloth
- warming
- fabric
- dreamlike
- change function
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention relates to interweaved fabric with a dreamlike color-change function and a preparation technology of the interweaved fabric, and belongs to the technical field of textile dyeing. The preparation technology comprises the following steps: preparing cloth; carrying out flat cylinder desizing; dyeing; carrying out color fixation; drying; sizing and carrying out finish inspection and packaging. The fabric prepared by the technology has a dual-color effect, and has the dreamlike color-change effect after being prepared into clothing; the fabric prepared according to the technology has excellent air permeability, comfortableness, abrasive resistance and color fastness; and the fabric surface is smooth and bright, is not easily stained, and is relatively good in stain resistance. In addition, the preparation technology disclosed by the invention is convenient to control, high in operability and suitable for large-scale popularization and application.
Description
Technical field
The invention belongs to technical field of textile printing, be specifically related to a kind of interwoven fabric and the manufacture craft thereof with dreamlike colour change function.
Background technology
Along with the continuous improvement of people's living condition, the requirement of people to dressing fabric is also more and more higher, not only requires that fabric has the physical properties such as certain cold-proof comfort, gas permeability, also requires that fabric has excellent chromaticity.And current fabric is when dyeing, mostly can only give the single colour system that fabric is traditional, namely a kind of fabric can only have a kind of color after once dyeing, and a lot of fabric after dyeing, though through fixation treatment, but its COLOR FASTNESS is still poor, polychrome washing and the rear color of use will be dim, even occur the phenomenon that fades during washing.
Therefore a kind of research with the interwoven fabric of dreamlike colour change function collecting excellent breathability, comfortableness, ABRASION RESISTANCE and look rigidity is just seemed particularly important.
Summary of the invention
The object of the invention is to overcome the deficiencies in the prior art and a kind of interwoven fabric and the manufacture craft thereof with dreamlike colour change function are provided, adopt the fabric that present invention process makes, there is two-color effect, after making ready-made clothes, there is the color changeable effect of illusion, and according to the fabric that this technique makes, there is excellent gas permeability, comfortableness, ABRASION RESISTANCE and look rigidity, cloth cover smooth.
The present invention adopts following technical scheme:
There is the manufacture craft of the interwoven fabric of dreamlike colour change function, comprise the steps:
Step one, joins cloth: clot is batched, and with the operation of " A " word car, often props up cloth and tears the leftover of bolt of cloth, ensures that cloth cloth cover is smooth;
Step 2, flat cylinder destarch:
1. 75-80 DEG C of laggard cloth is warming up to after entering water in cylinder;
2. each 30y selvage guide is accessed at two;
3. according to watermeter in cylinder, add liquid caustic soda 24-26 ɡ/L, refining agent 14-16 ɡ/L, degreaser 7-8 ɡ/L successively, stir;
4. be warming up to 94-96 DEG C, contaminate once with the speed of 90m/min, time 24-27min;
5. continue to be warming up to 108-112 DEG C, contaminate six times with the speed of 90m/min, time 2-3h;
6. be cooled to 30-35 DEG C, after draining, back into water, be warming up to 90-100 DEG C of washing 4 times, time 1-2h;
Step 3, dyeing:
1. enter water in dye vat, be warming up to 55-65 DEG C, according to watermeter, add levelling agent 14-16 ɡ/L, after cloth is contaminated 1 time with the speed of 90m/min, time 20-30min;
2. add the DISPERSE DYES of fabric weight 2%-4% again, cloth is contaminated once with the speed of 90m/min, time 20-30min; Wherein, after described DISPERSE DYES first uses the water-soluble solution of 40-45 DEG C, then add in dye vat;
3. add the ACID DYES of fabric weight 2%-4% again, cloth is contaminated once with 90m/min, time 20-30min;
4. be warming up to 68-72 DEG C, contaminate once with 90m/min;
5. be warming up to 78-82 DEG C, contaminate once with 90m/min;
6. be warming up to 93-97 DEG C, contaminate once with 90m/min;
7. be warming up to 108-112 DEG C, contaminate once with 90m/min;
8. be warming up to 118-122 DEG C, contaminate six times with 90m/min, time 2-3h;
Step 4, fixation:
1. be cooled to 80 DEG C, draining after checking colors, reenter water to 700L, by cloth with 90m/min washing once, time 23-27min, rear draining;
2. continue to be warming up to 85 DEG C, according to watermeter, add color-fixing agent 23-26 ɡ/L, cloth is soaked 4 times with the speed of 90m/min, time 1-2h, after go out cloth;
Step 5, dries: after clear water washing, cross drying machine drying, speed is not higher than 90m/min, and steam pressure 1kg, makes cloth cover half-dried, do not drip, and makes " A " word car and batch; Guarantee cloth cover is wrinkle resistant;
Step 6, sizing:
1. with temperature 168-172 DEG C, speed 60m/min, for fabric width 150cm, overfeeding 3%, to cloth cover sizing, makes " A " word car and batches;
2. according to mass percent, waterproofing agent 2.5-3.5%, softener 2.5-3.5% and water are added in liquid bath simultaneously and stir, wherein, waterproofing agent, softener and water amount to 100%, then liquid bath crossed by the cloth after fixation being dried, and shapes with the speed of 60m/min;
Step 7, becomes inspection packaging: test after classification to step 6 gained cloth and pack, have the interwoven fabric of dreamlike colour change function described in obtaining.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein cloth described in step one is the interwoven fabric of nylon and terylene.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein refining agent described in step 2 is fatty alcohol ether phosphoric acid ester, and described degreaser is dodecyl alcohol.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein levelling agent described in step 3 is fatty alcohol-polyoxyethylene ether, and described DISPERSE DYES is o-phenyl phenol, and described ACID DYES is benzoquinones base polymer.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein ACID DYES described in step 3 first uses water-soluble solution, after being heated to 85-95 DEG C, then adds in dye vat.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein color-fixing agent described in step 4 is phenol sulfonic formaldehyde condensation compound.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein waterproofing agent described in step 6 is perfluoroalkyl compound, and described softener is amino silicones.
Further, the described manufacture craft with the interwoven fabric of dreamlike colour change function, wherein dries described in step 5 and adopts roller drying machine to dry.
The present invention also provides a kind of interwoven fabric with dreamlike colour change function obtained by described manufacture craft.
The present invention compared with prior art, has following beneficial effect:
The first, the present invention, by joining the steps such as cloth, flat cylinder destarch, dyeing, fixation, oven dry and sizing, makes the fabric obtained not only have double-colored dreamlike effect, also gives the gas permeability of fabric excellence, comfortableness, ABRASION RESISTANCE and look rigidity; Especially in flat cylinder Desizing Step, considerable influence is had to the performance of fabric to the setting and selecting of auxiliary agent of interpolation that process parameter, fabric is more easily painted when dyeing, can effectively prevent the leftover of bolt of cloth cloth tail from occurring aberration, and, effectively can ensure according to the control adding opportunity and addition of the temperature in dyeing course of the present invention, time and dyestuff the uniformity that fabric is painted, during fixation, when color-fixing agent and fixation, the setting of each parameter effectively can ensure the look rigidity of fabric;
The second, the present invention is with the interwoven fabric of nylon and terylene for raw material cloth, and obtained fabric not only has two-color effect, and cloth cover smooth, and after being made as ready-made clothes, design on fabric surface not easily stains, and resistance to soiling is better;
3rd, manufacture craft of the present invention is convenient to control, workable, is suitable for applying on a large scale.
Detailed description of the invention
Below by detailed description of the invention, the present invention is described in further detail, but it will be understood to those of skill in the art that the following example only for illustration of the present invention, and should not be considered as limiting scope of the present invention.
embodiment 1
There is the manufacture craft of the interwoven fabric of dreamlike colour change function, comprise the steps:
Step one, joins cloth: clot is batched, and with the operation of " A " word car, often props up cloth and tears the leftover of bolt of cloth, and ensure that cloth cloth cover is smooth, described cloth is the interwoven fabric of nylon and terylene;
Step 2, flat cylinder destarch:
1. 80 DEG C of laggard cloth are warming up to after entering water in cylinder;
2. each 30y selvage guide is accessed at two;
3. according to watermeter in cylinder, add liquid caustic soda (NaOH) 25 ɡ/L, refining agent (fatty alcohol ether phosphoric acid ester) 15 ɡ/L, degreaser (dodecyl alcohol) 7.5 ɡ/L successively, stir;
4. be warming up to 95 DEG C, contaminate once with the speed of 90m/min dye jigger, time 25min;
5. continue to be warming up to 110 DEG C, contaminate six times with the speed dye jigger of 90m/min, time 2.5h;
6. be cooled to 33 DEG C, after draining, back into water, be warming up to 95 DEG C of washings 4 times, time 1.5h;
Step 3, dyeing:
1. enter water in dye vat, be warming up to 60 DEG C, according to watermeter, add levelling agent (fatty alcohol-polyoxyethylene ether) 15 ɡ/L, after cloth is contaminated 1 time with the speed dye jigger of 90m/min, time 25min;
2. add the DISPERSE DYES (o-phenyl phenol) of fabric weight 3% again, cloth is contaminated once with the speed of 90m/min dye jigger, time 25min; Wherein, after described DISPERSE DYES first uses the water-soluble solution of 43 DEG C, then add in dye vat;
3. add the ACID DYES (benzoquinones base polymer) of fabric weight 3% again, cloth is contaminated once with 90m/min dye jigger, time 25min;
4. be warming up to 70 DEG C, contaminate once with 90m/min dye jigger;
5. be warming up to 80 DEG C, contaminate once with 90m/min dye jigger;
6. be warming up to 95 DEG C, contaminate once with 90m/min dye jigger;
7. be warming up to 110 DEG C, contaminate once with 90m/min dye jigger;
8. be warming up to 120 DEG C, contaminate six times with 90m/min dye jigger, time 2.5h;
Step 4, fixation:
1. be cooled to 80 DEG C, draining after checking colors, reenter water to 700L, by cloth with 90m/min washing once, time 25min, rear draining;
2. continue to be warming up to 85 DEG C, according to watermeter, add color-fixing agent (phenol sulfonic formaldehyde condensation compound) 25 ɡ/L, cloth is soaked 4 times with the speed of 90m/min, time 1.5h, after go out cloth;
Step 5, dries: after clear water washing, cross drying machine drying, speed is not higher than 90m/min, and steam pressure 1kg, makes cloth cover half-dried, do not drip, and makes " A " word car and batch; Guarantee cloth cover is wrinkle resistant;
Step 6, sizing:
1. with temperature 170 DEG C, speed 60m/min, for fabric width 150cm, overfeeding 3%, to cloth cover sizing, makes " A " word car and batches;
2. according to mass percent, waterproofing agent (perfluoroalkyl compound) 5%, softener (amino silicones) 3% and water are added in liquid bath simultaneously and stirs, wherein, waterproofing agent, softener and water amount to 100%, liquid bath crossed by cloth after fixation being dried again, shapes with the speed of 60m/min;
Step 7, becomes inspection packaging: test after classification to step 6 gained cloth and pack, have the interwoven fabric of dreamlike colour change function described in obtaining.
embodiment 2
There is the manufacture craft of the interwoven fabric of dreamlike colour change function, comprise the steps:
Step one, joins cloth: clot is batched, and with the operation of " A " word car, often props up cloth and tears the leftover of bolt of cloth, and ensure that cloth cloth cover is smooth, described cloth is the interwoven fabric of nylon and terylene;
Step 2, flat cylinder destarch:
1. 75 DEG C of laggard cloth are warming up to after entering water in cylinder;
2. each 30y selvage guide is accessed at two;
3. according to watermeter in cylinder, add liquid caustic soda (NaOH) 24 ɡ/L, refining agent (fatty alcohol ether phosphoric acid ester) 14 ɡ/L, degreaser (dodecyl alcohol) 7 ɡ/L successively, stir;
4. be warming up to 94 DEG C, contaminate once with the speed of 90m/min dye jigger, time 27min;
5. continue to be warming up to 108 DEG C, contaminate six times with the speed dye jigger of 90m/min, time 3h;
6. be cooled to 30 DEG C, after draining, back into water, be warming up to 90 DEG C of washings 4 times, time 2h;
Step 3, dyeing:
1. enter water in dye vat, be warming up to 55 DEG C, according to watermeter, add levelling agent (fatty alcohol-polyoxyethylene ether) 14 ɡ/L, after cloth is contaminated 1 time with the speed dye jigger of 90m/min, time 30min;
2. add the DISPERSE DYES (o-phenyl phenol) of fabric weight 2% again, cloth is contaminated once with the speed of 90m/min dye jigger, time 30min; Wherein, after described DISPERSE DYES first uses the water-soluble solution of 40 DEG C, then add in dye vat;
3. add the ACID DYES (benzoquinones base polymer) of fabric weight 2% again, cloth is contaminated once with 90m/min dye jigger, time 30min;
4. be warming up to 68 DEG C, contaminate once with 90m/min dye jigger;
5. be warming up to 78 DEG C, contaminate once with 90m/min dye jigger;
6. be warming up to 93 DEG C, contaminate once with 90m/min dye jigger;
7. be warming up to 108 DEG C, contaminate once with 90m/min dye jigger;
8. be warming up to 118 DEG C, contaminate six times with 90m/min dye jigger, time 3h;
Step 4, fixation:
1. be cooled to 80 DEG C, draining after checking colors, reenter water to 700L, by cloth with 90m/min washing once, time 23min, rear draining;
2. continue to be warming up to 85 DEG C, according to watermeter, add color-fixing agent (phenol sulfonic formaldehyde condensation compound) 23 ɡ/L, cloth is soaked 4 times with the speed of 90m/min, time 2h, after go out cloth;
Step 5, dries: after clear water washing, cross drying machine drying, speed is not higher than 90m/min, and steam pressure 1kg, makes cloth cover half-dried, do not drip, and makes " A " word car and batch; Guarantee cloth cover is wrinkle resistant;
Step 6, sizing:
1. with temperature 168 DEG C, speed 60m/min, for fabric width 150cm, overfeeding 3%, to cloth cover sizing, makes " A " word car and batches;
2. according to mass percent, waterproofing agent (perfluoroalkyl compound) 2.5%, softener (amino silicones) 2.5% and water are added in liquid bath simultaneously and stirs, wherein, waterproofing agent, softener and water amount to 100%, liquid bath crossed by cloth after fixation being dried again, shapes with the speed of 60m/min;
Step 7, becomes inspection packaging: test after classification to step 6 gained cloth and pack, have the interwoven fabric of dreamlike colour change function described in obtaining.
embodiment 3
There is the manufacture craft of the interwoven fabric of dreamlike colour change function, comprise the steps:
Step one, joins cloth: clot is batched, and with the operation of " A " word car, often props up cloth and tears the leftover of bolt of cloth, and ensure that cloth cloth cover is smooth, described cloth is the interwoven fabric of nylon and terylene;
Step 2, flat cylinder destarch:
1. 78 DEG C of laggard cloth are warming up to after entering water in cylinder;
2. each 30y selvage guide is accessed at two;
3. according to watermeter in cylinder, add liquid caustic soda (NaOH) 26 ɡ/L, refining agent (fatty alcohol ether phosphoric acid ester) 16 ɡ/L, degreaser (dodecyl alcohol) 8 ɡ/L successively, stir;
4. be warming up to 96 DEG C, contaminate once with the speed of 90m/min dye jigger, time 24min;
5. continue to be warming up to 112 DEG C, contaminate six times with the speed dye jigger of 90m/min, time 2h;
6. be cooled to 35 DEG C, after draining, back into water, be warming up to 100 DEG C of washings 4 times, time 1h;
Step 3, dyeing:
1. enter water in dye vat, be warming up to 65 DEG C, according to watermeter, add levelling agent (fatty alcohol-polyoxyethylene ether) 16 ɡ/L, after cloth is contaminated 1 time with the speed dye jigger of 90m/min, time 20min;
2. add the DISPERSE DYES (o-phenyl phenol) of fabric weight 4% again, cloth is contaminated once with the speed of 90m/min dye jigger, time 20min; Wherein, after described DISPERSE DYES first uses the water-soluble solution of 45 DEG C, then add in dye vat;
3. add the ACID DYES (benzoquinones base polymer) of fabric weight 4% again, cloth is contaminated once with 90m/min dye jigger, time 20min;
4. be warming up to 72 DEG C, contaminate once with 90m/min dye jigger;
5. be warming up to 82 DEG C, contaminate once with 90m/min dye jigger;
6. be warming up to 97 DEG C, contaminate once with 90m/min dye jigger;
7. be warming up to 112 DEG C, contaminate once with 90m/min dye jigger;
8. be warming up to 122 DEG C, contaminate six times with 90m/min dye jigger, time 2h;
Step 4, fixation:
1. be cooled to 80 DEG C, draining after checking colors, reenter water to 700L, by cloth with 90m/min washing once, time 23min, rear draining;
2. continue to be warming up to 85 DEG C, according to watermeter, add color-fixing agent (phenol sulfonic formaldehyde condensation compound) 26 ɡ/L, cloth is soaked 4 times with the speed of 90m/min, time 1h, after go out cloth;
Step 5, dries: after clear water washing, cross drying machine drying, speed is not higher than 90m/min, and steam pressure 1kg, makes cloth cover half-dried, do not drip, and makes " A " word car and batch; Guarantee cloth cover is wrinkle resistant;
Step 6, sizing:
1. with temperature 172 DEG C, speed 60m/min, for fabric width 150cm, overfeeding 3%, to cloth cover sizing, makes " A " word car and batches;
2. according to mass percent, waterproofing agent (perfluoroalkyl compound) 3.5%, softener (amino silicones) 3.5% and water are added in liquid bath simultaneously and stirs, wherein, waterproofing agent, softener and water amount to 100%, liquid bath crossed by cloth after fixation being dried again, shapes with the speed of 60m/min;
Step 7, becomes inspection packaging: test after classification to step 6 gained cloth and pack, have the interwoven fabric of dreamlike colour change function described in obtaining.
Detected by the interwoven fabric that embodiment 1 to 3 gained has dreamlike colour change function, result is as shown in table 1 below:
Table 1 performance detection data
Note: CT is transverse breakage.
Claims (9)
1. there is the manufacture craft of the interwoven fabric of dreamlike colour change function, it is characterized in that, comprise the steps:
Step one, joins cloth: clot is batched, and with the operation of " A " word car, often props up cloth and tears the leftover of bolt of cloth, ensures that cloth cloth cover is smooth;
Step 2, flat cylinder destarch:
1. 75-80 DEG C of laggard cloth is warming up to after entering water in cylinder;
2. each 30y selvage guide is accessed at two;
3. according to watermeter in cylinder, add liquid caustic soda 24-26 ɡ/L, refining agent 14-16 ɡ/L, degreaser 7-8 ɡ/L successively, stir;
4. be warming up to 94-96 DEG C, contaminate once with the speed of 90m/min, time 24-27min;
5. continue to be warming up to 108-112 DEG C, contaminate six times with the speed of 90m/min, time 2-3h;
6. be cooled to 30-35 DEG C, after draining, back into water, be warming up to 90-100 DEG C of washing four times, time 1-2h;
Step 3, dyeing:
1. enter water in dye vat, be warming up to 55-65 DEG C, according to watermeter, add levelling agent 14-16 ɡ/L, after cloth is contaminated 1 time with the speed of 90m/min, time 20-30min;
2. add the DISPERSE DYES of fabric weight 2%-4% again, cloth is contaminated once with the speed of 90m/min, time 20-30min; Wherein, after described DISPERSE DYES first uses the water-soluble solution of 40-45 DEG C, then add in dye vat;
3. add the ACID DYES of fabric weight 2%-4% again, cloth is contaminated once with 90m/min, time 20-30min;
4. be warming up to 68-72 DEG C, contaminate once with 90m/min;
5. be warming up to 78-82 DEG C, contaminate once with 90m/min;
6. be warming up to 93-97 DEG C, contaminate once with 90m/min;
7. be warming up to 108-112 DEG C, contaminate once with 90m/min;
8. be warming up to 118-122 DEG C, contaminate six times with 90m/min, time 2-3h;
Step 4, fixation:
1. be cooled to 80 DEG C, draining after checking colors, reenter water to 700L, by cloth with 90m/min washing once, time 23-27min, rear draining;
2. continue to be warming up to 85 DEG C, according to watermeter, add color-fixing agent 23-26 ɡ/L, cloth is soaked four times with the speed of 90m/min, time 1-2h, after go out cloth;
Step 5, dries: after clear water washing, cross drying machine drying, speed is not higher than 90m/min, and steam pressure 1kg, makes cloth cover half-dried, do not drip, and makes " A " word car and batch; Guarantee cloth cover is wrinkle resistant;
Step 6, sizing:
1. with temperature 168-172 DEG C, speed 60m/min, for fabric width 150cm, overfeeding 3%, to cloth cover sizing, makes " A " word car and batches;
2. according to mass percent, waterproofing agent 2.5-3.5%, softener 2.5-3.5% and water are added in liquid bath simultaneously and stir, wherein, waterproofing agent, softener and water amount to 100%, then liquid bath crossed by the cloth after fixation being dried, and shapes with the speed of 60m/min;
Step 7, becomes inspection packaging: test after classification to step 6 gained cloth and pack, have the interwoven fabric of dreamlike colour change function described in obtaining.
2. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, cloth described in step one is the interwoven fabric of nylon and terylene.
3. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, refining agent described in step 2 is fatty alcohol ether phosphoric acid ester, and described degreaser is dodecyl alcohol.
4. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, levelling agent described in step 3 is fatty alcohol-polyoxyethylene ether, and described DISPERSE DYES is o-phenyl phenol, and described ACID DYES is benzoquinones base polymer.
5. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, ACID DYES described in step 3 first uses water-soluble solution, after being heated to 85-95 DEG C, then adds in dye vat.
6. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, color-fixing agent described in step 4 is phenol sulfonic formaldehyde condensation compound.
7. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, waterproofing agent described in step 6 is perfluoroalkyl compound, and described softener is amino silicones.
8. the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1, is characterized in that, dries and adopt roller drying machine to dry described in step 5.
9. the interwoven fabric with dreamlike colour change function obtained by the manufacture craft with the interwoven fabric of dreamlike colour change function according to claim 1.