CN105256616B - 一种提高真丝染色性能的方法 - Google Patents

一种提高真丝染色性能的方法 Download PDF

Info

Publication number
CN105256616B
CN105256616B CN201510799159.9A CN201510799159A CN105256616B CN 105256616 B CN105256616 B CN 105256616B CN 201510799159 A CN201510799159 A CN 201510799159A CN 105256616 B CN105256616 B CN 105256616B
Authority
CN
China
Prior art keywords
silk
residue
dyeing performance
drying
pidolidone
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201510799159.9A
Other languages
English (en)
Other versions
CN105256616A (zh
Inventor
韦信礼
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangzhou Moses dikeni clothing Limited by Share Ltd
Original Assignee
Guangzhou Moses Dikeni Clothing Ltd By Share Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangzhou Moses Dikeni Clothing Ltd By Share Ltd filed Critical Guangzhou Moses Dikeni Clothing Ltd By Share Ltd
Priority to CN201510799159.9A priority Critical patent/CN105256616B/zh
Publication of CN105256616A publication Critical patent/CN105256616A/zh
Application granted granted Critical
Publication of CN105256616B publication Critical patent/CN105256616B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种提高真丝染色性能的方法,其充分利用多种手段结合,尤其是蛋白质和多糖的使用,超声波手段的引入,无化学物质残留,天然环保,无需高温,并且处理后的真丝具有优异的染色性能以及抗皱性。

Description

一种提高真丝染色性能的方法
技术领域
本发明涉及一种提高真丝染色性能的方法,属于纺织领域。
背景技术
真丝织物具有光泽柔和、手感柔滑、吸湿透气等优良的服用性能,特别适宜于制作对抗菌性有较高要求的内衣和婴幼儿服装等产品。蚕丝织物因具有吸湿快干、优雅光泽和滑爽的手感而受到人们的喜爱。理论上蚕丝织物可以用酸性、中性、直接、活性、阳离子、还原、可溶性还原、不溶性偶氮染料染色,但实际应用中,因丝纤维在碱性介质中容易受损,所以一般以酸性染料染色为主一,辅以中性、直接、活性染料染色。蚕丝纤维用匀染性酸性染料染色时湿牢度较差,织物染深性不好,染色脚水对环境污染严重,所以提高蚕丝纤维染色性能具有重要意义。
本发明旨在提供一种提高真丝染色性能的方法,其充分利用多种手段结合,尤其是蛋白质和多糖的使用,超声波手段的引入,无化学物质残留,天然环保,无需高温,并且处理后的真丝具有优异的染色性能以及抗皱性。
发明内容
基于背景技术存在的技术问题,本发明针对背景技术存在的问题,提供一种提高真丝染色性能的方法,其充分利用多种手段结合,尤其是蛋白质和多糖的使用,超声波手段的引入,无化学物质残留,天然环保,无需高温,并且处理后的真丝具有优异的染色性能以及抗皱性。
本发明的目的通过以下技术方案实现:
一种提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温60-65℃处理,然后用去离子水清洗干净残留物,40-45℃烘干;
所述预处理液配方为:褐藻糖胶0.05-0.08%,大豆蛋白0.5-0.8%,L-谷氨酸0.15-0.25%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸2-5min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理3-5min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.6-0.9%,L-谷氨酸0.3%,苹果酸0.2-0.4%。
本发明的有益之处在于:
本发明提供一种提高真丝染色性能的方法,其充分利用多种手段结合,尤其是蛋白质和多糖的使用,超声波手段的引入,无化学物质残留,天然环保,无需高温,并且处理后的真丝具有优异的染色性能以及抗皱性。
具体实施方式
本发明所用的真丝织物均为真丝绸14654素绉缎试样。
实施例1:
提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温60℃处理,然后用去离子水清洗干净残留物,45℃烘干;
所述预处理液配方为:褐藻糖胶0.05%,大豆蛋白0.8%,L-谷氨酸0.15%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸5min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理3min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.9%,L-谷氨酸0.3%,苹果酸0.2%。
实施例2:
提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温65℃处理,然后用去离子水清洗干净残留物,40℃烘干;
所述预处理液配方为:褐藻糖胶0.08%,大豆蛋白0.5%,L-谷氨酸0.25%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸2min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理5min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.6%,L-谷氨酸0.3%,苹果酸0.4%。
实施例3:
提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温61℃处理,然后用去离子水清洗干净残留物,44℃烘干;
所述预处理液配方为:褐藻糖胶0.06%,大豆蛋白0.7%,L-谷氨酸0.20%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸4min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理4min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.8%,L-谷氨酸0.3%,苹果酸0.3%。
实施例4:
提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温64℃处理,然后用去离子水清洗干净残留物,41℃烘干;
所述预处理液配方为:褐藻糖胶0.07%,大豆蛋白0.6%,L-谷氨酸0.19%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸3min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理3min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.7%,L-谷氨酸0.3%,苹果酸0.4%。
实施例5:
提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温62℃处理,然后用去离子水清洗干净残留物,43℃烘干;
所述预处理液配方为:褐藻糖胶0.05%,大豆蛋白0.8%,L-谷氨酸0.21%,
所述大豆蛋白的分子量为5000道尔顿;
(2)将预处理后的真丝用蒸汽均匀熏蒸5min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理4min,然后用去离子水清洗干净残留物,50℃烘干既得。
所述处理液配方为:海藻糖1%,水溶性硅油0.9%,L-谷氨酸0.3%,苹果酸0.2%。
实施例6:
效果测评:
酸性大红3R染色工艺进行染色性能测评:
染色工艺:在50℃入染,10min后以10℃/min升温速度升温至90℃,保温染色60min后降温、排液、后处理。
染色处方:
酸性染料 2%o.w.f.;
硫酸钠 1g/L;
pH 4.0;
浴比 100:1
K/S值测试:织物折叠2层,在DataC olor650测色配色仪上测定K/S值,取四个不同的点测定,取平均值。
皂洗牢度的评定:参照GB/T3921.1-1997测试。
实验结果如下表所示:
表1
此检测数据只针对上述检测样品。
由此可见,本发明提供一种提高真丝染色性能的方法,其充分利用多种手段结合,尤其是蛋白质和多糖的使用,超声波手段的引入,无化学物质残留,天然环保,无需高温,并且处理后的真丝具有优异的染色性能以及抗皱性。
以上所述,仅为本发明较佳的具体实施方式,但本发明的保护范围并不局限于此,任何熟悉本技术领域的技术人员在本发明揭露的技术范围内,根据本发明的技术方案及其发明构思加以等同替换或改变,都应涵盖在本发明的保护范围之内。

Claims (2)

1.一种提高真丝染色性能的方法,其步骤如下:
以下均为质量百分比;
(1)将取真丝织物浸入预处理液中,浴比1:50,放入恒温超声波发生器中,保持恒温60-65℃处理,然后用去离子水清洗干净残留物,40-45℃烘干;
所述预处理液配方为:褐藻糖胶0.05-0.08%,大豆蛋白0.5-0.8%,L-谷氨酸0.15-0.25%;
(2)将预处理后的真丝用蒸汽均匀熏蒸2-5min;
(3)将熏蒸后的真丝浸入处理液中,浴比1:30,放入恒温超声波发生器中,保持恒温55℃处理3-5min,然后用去离子水清洗干净残留物,50℃烘干既得;
所述处理液配方为:海藻糖1%,水溶性硅油0.6-0.9%,L-谷氨酸0.3%,苹果酸0.2-0.4%。
2.权利要求1所述的提高真丝染色性能的方法,其特征在于:
所述大豆蛋白的分子量为5000道尔顿。
CN201510799159.9A 2015-11-18 2015-11-18 一种提高真丝染色性能的方法 Active CN105256616B (zh)