CN104643756B - 印花夜光毛毯、地毯及其生产工艺 - Google Patents

印花夜光毛毯、地毯及其生产工艺 Download PDF

Info

Publication number
CN104643756B
CN104643756B CN201510015675.8A CN201510015675A CN104643756B CN 104643756 B CN104643756 B CN 104643756B CN 201510015675 A CN201510015675 A CN 201510015675A CN 104643756 B CN104643756 B CN 104643756B
Authority
CN
China
Prior art keywords
stamp
luminous
carpet
woollen blanket
printing portion
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201510015675.8A
Other languages
English (en)
Other versions
CN104643756A (zh
Inventor
段云宝
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201510015675.8A priority Critical patent/CN104643756B/zh
Publication of CN104643756A publication Critical patent/CN104643756A/zh
Application granted granted Critical
Publication of CN104643756B publication Critical patent/CN104643756B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了印花夜光毛毯、地毯及其生产工序,所述毛毯/地毯本体上设置有夜光印花部。印花夜光毛毯/地毯生产工艺,包括制图、白胚织造、印花、固色、柔软处理、烘干定型、后整理处理步骤,所述印花步骤包括常规印花部印花、夜光印花部印花、渗透步骤,所述夜光印花部印花所用浆料配制特别;所述固色步骤包括先进行不低于150℃高温烘干,再进行常规高温高压汽压蒸化,其余工序按常规进行,所得的印花夜光毛毯/地毯形成局部图案或全部图案的夜光印花部,印花牢固,不退色,易于清理,且毛毯、地毯表面柔软度不受任何影响,同时在常规的印花毛毯、地毯生产工艺中略作调整,工艺简单。

Description

印花夜光毛毯、地毯及其生产工艺
技术领域
本发明涉及毛毯、地毯领域,具体涉及印花夜光毛毯、地毯及其生产工艺。
背景技术
毛毯、地毯因其保暖、柔软舒适、大气上档次,为家居、高档宾馆热衷选用。目前市场上已有开发夜光毛毯、地毯,夜晚时依然可以展示毛毯、地毯的精美图案,同时也可在黑夜中起到指示位置的作用。但市场上的夜光毛毯、地毯或是在其中加设电子发光器件,或在毛毯、地毯本体表面设置发光物质层。加设电子发光器件需要防水、防潮,工艺复杂且易损坏,不利于清洗;表层设置发光物质的夜光毛毯、地毯,降低了毯子的表面柔软性,且发光物质容易掉落,也不耐洗。
发明内容
本发明要解决的技术问题是提供一种印花夜光毛毯、地毯及其生产工艺,通过印花工艺将发光物质连同染料一并渗透、印制于本体内,形成局部图案或全部图案的夜光印花部,印花牢固,不退色,表面柔软度不受任何影响,在常规的印花毛毯、地毯生产工艺中略作调整,工艺简单。
本发明通过以下技术方案实现:
印花夜光毛毯、地毯,所述毛毯/地毯本体上设置有夜光印花部。
本发明进一步改进方案是,所述毛毯/地毯本体采用DTY面纱和FDY底丝织造而成。
本发明生产工艺技术方案:
印花夜光毛毯、地毯生产工艺,包括制图、白胚织造、印花、固色、柔软处理、烘干定型、后整理处理步骤,所述印花步骤包括常规印花部印花、夜光印花部印花、渗透步骤,所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2~3%、丙烯酸脂8~10%、2000~2500目油性夜光粉4~6%、荧光染料1~2%、水80~85%;所述固色步骤包括先进行不低于150℃高温烘干至产品含水率≤2%,再进行常规高温高压汽压蒸化。
本发明进一步改进方案是,所述印花步骤中温度为130~135℃,压力为3kg/cm2
本发明更进一步改进方案是,所述固色步骤中常规高温高压汽压蒸化的温度为130℃,压力为3kg/cm2
本发明与现有技术相比,具有以下明显优点:
本发明通过调制夜光印染特殊浆料,在毛毯/地毯的印花工序中增加一道夜光印花部印花,将常规印花部印花和夜光印花部印花分两道印花;同时其后序的固色工序中先进行不低于150℃高温烘干至产品含水率≤2%,再进行常规高温高压汽压蒸化,其他工序按常规工艺处理,所得的印花夜光毛毯/地毯形成局部图案或全部图案的夜光印花部,丙烯酸脂的加入将夜光粉、荧光染料牢牢地吸附在毛毯/地毯本体纤维内,且柔软度不受任何影响,夜光印花吸附牢固,不退色,易于清理,柔软舒适;同时仅在常规的印花毛毯/地毯生产工艺中略作调整,工艺简单。
附图说明
图1为印花夜光地毯。
具体实施方式
实施例1
如图1所示,本发明所述的印花夜光地毯本体1上设置有夜光印花部2(星星部位)。
印花夜光地毯生产工艺:
一、制图
1)电脑分色;
2)电脑出胶片;
3)感光制版;
4)印花网版成型;
二、织造
1)DTY面纱与FDY底丝编织成白胚;
2)白胚定型;
3)白胚整理;
三、印花
1)常规印花部印花(除星星图案以外的其它部位印花成浅蓝色);
2)夜光印花部印花(星星图案部位印花成金色,夜晚可以发光);
夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2.5%、丙烯酸脂8%、2500目油性夜光粉5%、荧光染料1%、水83.5%;
常规印花部印花与夜光印花部印花工序中温度为132℃,压力3kg/cm2
3)常温常压下渗透机渗透;
四、固色
1)150℃烘干至产品含水率≤2%,保证夜光印花部印花浆料牢固固色,附着于白胚纤维内;
2)常规130℃、压力3kg/cm2汽压蒸化;
五、柔软处理
1)水洗处理;
2)柔软剂处理;
六、烘干定型
七、后整理处理
1)梳毛处理;
2)烫光处理;
八、成品作业
1)与海绵无纺布贴合;
2)根据需要尺寸裁剪;
3)包边;
4)检验;
5)包装。
实施例2
所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2%、丙烯酸脂10%、2000目油性夜光粉4%、荧光染料1.5%、水82.5%;
常规印花部印花与夜光印花部印花工序中温度为130℃,压力3kg/cm2
所述固色工序中烘干温度为160℃。
其余如实施例1。
实施例3
所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂3%、丙烯酸脂9%、2500目油性夜光粉6%、荧光染料2%、水80%;
常规印花部印花与夜光印花部印花工序中温度为135℃,压力3kg/cm2
所述固色工序中烘干温度为135℃。
其余如实施例1。
三个实施例制成的夜光毛毯,常规印花部与夜光印花部表面柔软,无差异;在夜晚无光亮的情况下,夜光印花部的图案清晰可见。

Claims (7)

1.印花夜光毛毯,其特征在于:所述毛毯本体上设置有夜光印花部;
印花夜光毛毯生产工艺,包括制图、白胚织造、印花、固色、柔软处理、烘干定型、后整理处理步骤,所述印花步骤包括常规印花部印花、夜光印花部印花、渗透步骤,所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2~3%、丙烯酸脂8~10%、2000~2500目油性夜光粉4~6%、荧光染料1~2%、水80~85%;所述固色步骤包括先进行不低于150℃高温烘干至产品含水率≤2%,再进行常规高温高压汽压蒸化。
2.根据权利要求1所述的印花夜光毛毯,其特征在于:所述毛毯本体采用DTY面纱和FDY底丝织造而成。
3.印花夜光地毯,其特征在于:所述地毯本体上设置有夜光印花部;
印花夜光地毯生产工艺,包括制图、白胚织造、印花、固色、柔软处理、烘干定型、后整理处理步骤,所述印花步骤包括常规印花部印花、夜光印花部印花、渗透步骤,所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2~3%、丙烯酸脂8~10%、2000~2500目油性夜光粉4~6%、荧光染料1~2%、水80~85%;所述固色步骤包括先进行不低于150℃高温烘干至产品含水率≤2%,再进行常规高温高压汽压蒸化。
4.根据权利要求3所述的印花夜光地毯,其特征在于:所述地毯本体采用DTY面纱和FDY底丝织造而成。
5.印花夜光毛毯、地毯生产工艺,包括制图、白胚织造、印花、固色、柔软处理、烘干定型、后整理处理步骤,其特征在于:所述印花步骤包括常规印花部印花、夜光印花部印花、渗透步骤,所述夜光印花部印花所用浆料由以下重量份组分混合而成:增稠剂2~3%、丙烯酸脂8~10%、2000~2500目油性夜光粉4~6%、荧光染料1~2%、水80~85%;所述固色步骤包括先进行不低于150℃高温烘干至产品含水率≤2%,再进行常规高温高压汽压蒸化。
6.根据权利要求5所述的印花夜光毛毯、地毯生产工艺,其特征在于:所述印花步骤中温度为130~135℃,压力为3kg/cm2
7.根据权利要求5所述的印花夜光毛毯、地毯生产工艺,其特征在于:所述固色步骤中常规高温高压汽压蒸化的温度为130℃,压力为3kg/cm2
CN201510015675.8A 2015-01-13 2015-01-13 印花夜光毛毯、地毯及其生产工艺 Expired - Fee Related CN104643756B (zh)